Clogged nozzle? Clear it in the right order and stop it coming back
By Sina Esfahani, OmniTechs · Published 27 November 2026
A clogged nozzle shows in two ways. With a full clog nothing comes out. With a partial clog some plastic gets through, but lines are thin, layers have gaps, purged filament curls up and the extruder often clicks.
Pick the method by whether the filament still moves. If it loads and unloads but prints badly, do a cold pull. If nothing comes out, heat higher and push fresh filament through, then try the needle. If that fails, the plug sits higher up or the nozzle is due for replacement. A clogged hotend is not always a clogged nozzle: the blockage can sit in the PTFE tube or heatbreak, so a new nozzle is not a guaranteed fix (Prusa).
Fix it in this order:
Unload the filament, raise the nozzle and put on heat-resistant gloves.
Purge at print temperature: a straight, smooth strand means no clog; a thin or curling one means a partial clog.
Partial clog: do a cold pull with PLA (Prusa: fill at 270 °C, pull at 85 to 100 °C; Bambu Lab: 220 °C and 100 °C).
Nothing comes out: heat to 260 °C after PLA or 280 °C after PETG, ABS or ASA, wait 2 minutes and push fresh PLA by hand.
Particles at the tip: pass the needle 1 to 2 cm in from below at temperature, never on 0.2 mm or high-flow nozzles.
Still blocked: switch off, unplug and let it cool, then look for the plug higher up or replace the nozzle.
After any nozzle work, check it is tight and redo the first-layer calibration.
What you see and what it means
Clog symptoms: what you see, what it means, what to do
| What you see | What it means | What to do |
|---|---|---|
| Nothing comes out and the extruder clicks loudly | A full clog, or a deformed nozzle | Heat higher and push fresh filament; then the needle |
| Thin, uneven lines; the purged strand curls and sticks to the nozzle | A partial clog, often particles at the tip | Cold pull; the needle for particles |
| A short, rough strand when you extrude PLA at 220 °C | A narrowed nozzle or a faulty drive gear | Push PLA into the nozzle by hand to tell them apart |
| Prints well, then stops about the same time into every print | Heat creep rather than an ordinary clog | Fix cooling and enclosure temperature first |
| A wire pushed in from above stops well above the tip | The plug sits in the PTFE tube or heatbreak | Remove the hotend and pull the plug out at temperature |
| Plastic leaking around the nozzle threads | The nozzle does not seal against the heatbreak | Hot-tighten the nozzle |
| Only the first layer is thin, the nozzle sits against the plate | Not a clog: the nozzle is too close | Raise the z-offset |
Start with the sound: a loud click most likely means a clogged or deformed nozzle, a light click points to the gears (Prusa). Then check that the filament actually reaches the gear. Bambu Lab's free-air test settles the rest: at 220 °C, PLA that drops long, smooth and straight means the nozzle and gear are fine. A first layer set too close is covered in setting the z-offset, and a jam that builds up after normal printing in heat creep explained.
Which method to use: the makers disagree
Prusa and Bambu Lab ship a cleaning needle with their printers. E3D lists the needle as a method it does not recommend for its V6 nozzles. Follow the maker of the nozzle you actually have.
Who recommends which cleaning method
| Method | E3D (V6 brass nozzle) | Prusa | Bambu Lab |
|---|---|---|---|
| Needle or pin through the tip | Not recommended | Bundled 0.3 to 0.35 mm needle; not for high-flow nozzles | Bundled pin; skip on 0.2 mm (X1, P1), not below 0.4 mm (A1) |
| Cold pull | Recommended | Recommended for partial clogs, with PLA | Recommended, at least once a month |
| Nylon cleaning filament | Recommended; the only method for Nozzle X | Use only cleaning filament on Nozzle X | Not covered |
| Brass brush outside | Recommended; steel wire brushes not | Not covered | Not covered |
| Blow torch | Not recommended | Not covered | Not covered |
3D Printing Nerd shows the cleaning-filament route: a cold pull with nylon to clear debris that causes inconsistent extrusion.
Nothing comes out: heat higher and push
Turn off filament autoload (Prusa) so the printer does not fight you.
Set 260 °C if you last printed PLA, or 280 °C after PETG, ABS or ASA. On an MK3 the path is LCD Menu → Settings → Temperature → Nozzle; on Nextruder printers LCD Menu → Control → Temperature → Nozzle.
Wait 2 minutes; the filament should start to drip.
Open the idler and push about 40 cm of fresh PLA in by hand (Prusa's Nextruder guide).
If flow does not return, the blockage sits further up. Prusa then expects a cold pull to fail too, and on Nextruder printers says the nozzle most likely needs replacing. On Nextruder printers, heat the nozzle only through the printer's menu, never with an external heat source (Prusa).
Particles at the tip: the needle
Particles from carbon fibre, glow-in-the-dark or sparkle filament can be larger than the nozzle hole and block it (Bambu Lab). The needle dislodges them:
Heat the nozzle. Bambu Lab uses 250 °C, which it says suits PLA, PETG, TPU and ABS; on the X1 and P1 the setting is under Settings → Temperature/Axis.
Push the needle 1 to 2 cm in from below and move it a few times (Prusa). Never feed it in from the top, and on the MK3 do not load filament with the needle in.
Do not push it too far, or you force molten plastic higher up and make the clog harder to remove (Bambu Lab).
Wear heat-resistant gloves and keep your face away. Pressure built up behind a clog can make molten filament spray out suddenly (Bambu Lab).
Then extrude again: the strand should come out straight, not curled.
Partial clog: the cold pull, step by step
A cold pull fills the nozzle with PLA, lets it cool until it is almost solid and pulls it out with the dirt on its tip. Prusa says PLA works best; other filaments tear or melt too much. The temperatures differ per printer.
Cold-pull temperatures published by the makers
| Printer | Fill with PLA at | Pull at |
|---|---|---|
| Prusa MK3S, MK3.5 | 270 °C | 85 °C, after cooling to room temperature first |
| Prusa CORE One, MK4, XL (manual) | 270 °C | 100 °C on the way down |
| Prusa CORE One, MK4/S, MK3.9/S, XL (automatic, Control → Cold Pull) | Printer waits until 36 °C | 80 °C, unloaded by the printer |
| Bambu Lab X1, P1 and A1 | 220 °C | 100 °C |
Open the extruder or remove the PTFE tube so you can feed by hand, and turn off filament sensing or autoload where the maker says so.
Heat to the fill temperature and push PLA in until it flows out of the nozzle.
Stop heating and keep pushing as it cools, until it no longer comes out (around 170 °C for PLA, Prusa). The nozzle must stay full. Pick the plastic from under the tip.
At the pull temperature, pull slowly and steadily, straight up. On Bambu Lab printers press retract and only help gently by hand.
Dark marks or another colour on the tip mean repeat. A clean tip carrying the imprint of the nozzle means the job is done (Prusa).
Afterwards, re-enable the filament sensor and run the Z or first-layer calibration (Prusa). Bambu Lab's own video shows the whole cold pull with PLA on its printers.
When the plug sits higher up
Switch the printer off, unplug it and let it cool before you take the hotend apart, as Bambu Lab instructs for all maintenance. When you heat a removed hotend again, hold it only with heat-resistant gloves and keep anything flammable away from it (Bambu Lab).
On an MK3, a 1.5 mm wire pushed in from the top shows how deep the plug starts (Prusa).
Filament stuck in the PTFE tube: remove the hotend, heat it back to 260 or 280 °C and pull the filament up with pliers (Prusa). On Nextruder printers Prusa grips visible filament at 280 °C and feeds it up bit by bit.
A PTFE tube damaged by the clog must be replaced and locked in place: pull the collet up about 1 mm while pushing the tube down (Prusa). Any gap between tube and metal lets filament bulge and jam (Teaching Tech).
With the nozzle out, push or extrude filament through the empty hotend to confirm the rest of the path is clear (an accepted answer on the 3D Printing Stack Exchange).
Tighten or replace the nozzle
A nozzle that does not seal against the heatbreak leaks around the threads and clogs again. On V6-style hotends the nozzle must be tightened hot, with a gap of about 0.5 mm left to the heater block (Prusa). E3D's procedure for a brass V6 nozzle: heat to 285 °C, wait about a minute, then tighten with a 7 mm spanner and an adjustable wrench to 2 Nm. Too much force can shear the nozzle or heatbreak, so E3D suggests a torque wrench. Keep your fingers off the heater block and wear heat-resistant gloves, as Bambu Lab asks whenever you handle a hot hotend. Its other nozzle materials are tightened at 20 °C above your print temperature. On Nextruder printers, push the nozzle up until the copper ring disappears and tighten the thumb screws by hand only (Prusa).
Replace rather than clean when the nozzle is old or heavily used (Prusa), or when cleaning fails (Bambu Lab). After a nozzle change, redo at least the first-layer calibration. Nozzle materials and threads are compared in nozzle types.
Prevent the next clog
Purge when you change material. After a hotter material, load the new one at the old, higher temperature (Prusa).
Do a cold pull at least once a month, especially when you switch filament types (Bambu Lab).
Do not leave a hot nozzle idle: filament degrades, hardens and blocks the tip (Teaching Tech). Combine short jobs into one print (Bambu Lab).
Use 0.6 or 0.8 mm nozzles for fibre-filled filament, never 0.2 mm (Bambu Lab); see carbon fibre filament.
Keep filament dry and within tolerance; Bambu Lab checks for 1.75 ±0.03 mm. See signs of wet filament.
Keep retraction modest: too much with PLA pulls softened plastic up to where it sets (3D Printing Stack Exchange).
Do not set the first layer so close that it presses the nozzle into the plate; Prusa links that to clogs.
Keep the silicone sock on the heater block: it steadies the nozzle temperature and reduces build-up (Bambu Lab).
Worked example: back to PLA after a carbon-filled nylon
Bambu Lab's sequence after a high-temperature material such as PAHT-CF:
Heat the nozzle to 250 to 300 °C.
Unload the high-temperature filament.
Load the PLA and let it push the residue out.
Keep extruding while you lower the nozzle to 220 to 240 °C, until the PLA flows clean and steady.
If it still will not flow, raise the temperature further and use the needle (Bambu Lab).
When to stop, and where to go next
Stop and replace the part when a cold pull and the push-through both fail. On Nextruder printers that usually means a new nozzle; on Bambu Lab printers a new hotend if it cannot be unclogged. A dented nozzle tube on the XL needs replacing too (Prusa). If heating never brings the plastic to flow, the heater may be ageing (Bambu Lab). Contact the maker's support with photos of the cold-pull tip.
If the clog keeps coming back, find out why. Heat creep explained covers jams above the melt zone, and under-extrusion causes and fixes the other reasons plastic goes missing. If you need the part rather than the practice, the 3D printing service prints PLA and PETG parts from your file.
Sources
Prusa Knowledge Base: Clogged nozzle/hotend (MK3.5/S, MK3S, MK2.5S)
Prusa Knowledge Base: Clogged nozzle (CORE One, XL, MK4/S, MK3.9/S)
Prusa Knowledge Base: Cold pull (MK4/S, MK3.9/S, MK3.5/S, XL)
Bambu Lab Wiki: Troubleshooting Steps if Filament Not Extruding (X1, P1)
E3D: Classics support, V6 nozzle (hot tightening and cleaning)
3D Printing Stack Exchange: How do I keep my extruder head from getting clogged?
3D Printing Nerd: How to fix a clogged nozzle using a cold pull (YouTube)