3D printer under-extrusion: find the cause in seven checks

By Sina Esfahani, OmniTechs · Published 27 November 2026

Under-extrusion means less plastic leaves the nozzle than the slicer asked for. You see gaps between lines, thin or missing layers and walls that snap. The printer cannot measure its own output, so the shortfall can start anywhere between the spool and the nozzle tip (Prusa).

Most cases come down to one of three things: the filament meets resistance, the hotend cannot melt plastic as fast as the print demands, or a setting asks for the wrong amount. Check the quick, free things first and the hardware next. Change flow or e-steps last: a calibration made over a dirty extruder or a partial clog only bakes the fault into your settings (Bambu Lab).

Fix it in this order:

  1. Check the filament diameter in the slicer: 1.75 mm filament set as 2.85 mm delivers only about 38 % of the plastic.

  2. Turn the spool by hand and pull the filament through its tube: it must move without catching.

  3. Extrude with the nozzle raised: if plastic flows there but not on the first layer, raise the z-offset.

  4. Slow down where the gaps are: keep the flow 10 to 20 % below what your hotend can melt (OrcaSlicer).

  5. Purge and watch the strand: a thin or curling strand means a partial clog, so do a cold pull.

  6. Look at the extruder gears: plastic dust or a bite in the filament means slipping; clean and set the idler.

  7. Dry the spool if it pops or bubbles, and only then calibrate flow (typical values 0.9 to 1.1, Prusa).

What the pattern tells you

Where and when the gaps appear points to the cause before you touch anything.

Under-extrusion symptoms and what they mean

Compiled from the Bambu Lab Wiki under-extrusion and clog pages, the Prusa Knowledge Base under-extrusion articles and the Teaching Tech troubleshooting guide, read 27 November 2026.
What you seeWhat it meansWhat to do
Gaps everywhere from the first layer, on a new printer or new profileThe slicer thinks the filament is thicker than it is, or flow is far too lowSet the filament diameter to match the spool, then measure the filament
Thin, see-through or missing first layer, often with clickingThe nozzle is so close to the plate that plastic cannot get outRaise the z-offset and test extrusion in free air
Gaps in infill and fast sections, perimeters fineThe print asks for more plastic per second than the hotend can meltLower the speed or the maximum volumetric speed, or print hotter within the filament's range
Good at first, worse later, then nothingA partial clog or heat creepCheck the hotend fan, open the enclosure for PLA, do a cold pull
Gaps only at corners or after travel movesPressure advance or retraction, not a lack of plasticCalibrate pressure advance and check retraction
Plastic dust at the gear, a bite mark in the filamentThe gear slips against resistance further downClear the path first, then clean the gears and set the tension
Popping, bubbles, rough surface, stringingWet filamentDry the spool and print the same part again

Gaps everywhere from the start: the slicer and the first layer

When a new printer or a fresh profile under-extrudes everywhere, check the slicer before the hardware. A classic case on the 3D Printing Stack Exchange: a Cura profile left at 2.85 mm with 1.75 mm filament loaded. The slicer then thinks each millimetre of filament holds about 2.65 times more plastic than it does, so only about 38 % of the needed volume arrives. Even 130 % flow still looked spotty. The fix is the right diameter, not more flow.

Then measure the filament at a few points with a caliper. Prusa calls ±0.05 mm the industry standard; Bambu Lab's quality check asks for 1.75 ±0.03 mm. The 1.75 mm or 2.85 mm guide explains the two sizes.

If only the first layer is thin or missing, the nozzle is probably too low. Plastic has nowhere to go and the extruder may click. Bambu Lab's quick test: move the toolhead to the purge position, heat the nozzle and extrude. If it flows freely there but not on the plate, the nozzle is too close, or a loose hotend is being pushed down by the extrusion force. Do not fix poor adhesion by squashing the first layer harder (Prusa); set the gap with setting the z-offset.

Gaps in fast sections: the hotend's melt limit

A hotend can only melt so much plastic per second. Prusa calls this the maximum volumetric speed, in mm³/s, and names extruder clicking, under-extrusion at high speed and poor layer adhesion as signs that the limit is set too high. The print's demand is roughly line width × layer height × speed. Thick layers, wide lines and fast infill hit the limit first.

Melt limits the makers publish for their own hardware

From the E3D V6 nozzle support page, the Prusa maximum volumetric speed article and the Bambu Lab H2D extruder overload guide, read 27 November 2026. Each figure applies only to that maker's hardware and filament.
MakerHotend, nozzle and filamentPublished figure
E3DV6 with 0.4, 0.6 or 0.8 mm brass nozzle, PLA at 220 °C13, 14 or 15 mm³/s
PrusaStandard all-metal hotend such as the E3D V6 or stock MK38 to 12 mm³/s, typical
PrusaNextruder (MK4, XL)15 to 20 mm³/s, typical
Bambu LabPLA Basic preset, standard hotend (H2D)25 mm³/s
Bambu LabPLA Basic preset, high-flow hotend (H2D)35 mm³/s

Worked example: is 100 mm/s too fast for a V6?

A 0.45 mm line at 0.2 mm layers and 100 mm/s needs 0.45 × 0.2 × 100 = 9 mm³/s. That is under E3D's 13 mm³/s for a 0.4 mm V6 with PLA. Infill at 0.28 mm layers, 0.5 mm wide and 150 mm/s needs 0.5 × 0.28 × 150 = 21 mm³/s: far past the limit, so the infill shows gaps. The safe speed is the limit divided by the line's cross-section: 13 ÷ (0.5 × 0.28) is about 93 mm/s. With OrcaSlicer's advice to stay 10 to 20 % below the limit, set roughly 74 to 84 mm/s. (PrusaSlicer models the line with rounded sides, so its flow figures come out slightly lower; the rectangle errs on the safe side.)

Set or measure the limit

  • PrusaSlicer: Print Settings → Speed → Max volumetric speed, or Filament Settings → Advanced → Max volumetric speed; the lower of the two wins. The Volumetric flow rate preview shows where it bites.

  • OrcaSlicer: print the Max Volumetric Speed test from the Calibration menu (default 5 to 20 mm³/s in steps of 0.5). Note the height where the walls start to deform and work out start + height × step. In the wiki's example quality drops at 36 mm, so 5 + 36 × 0.5 = 23 mm³/s, and 20 mm³/s goes into the filament settings.

  • A high-flow nozzle needs a high-flow profile, and the other way round; a mismatch causes severe under-extrusion (Prusa) or an extruder overload error (Bambu Lab).

Temperature moves the limit. Stay inside the filament maker's range (Polymaker: 190 to 230 °C for PolyLite PLA). Hardened or stainless steel nozzles often need 5 to 10 °C more than brass, and an unlisted brand may need 5 to 15 °C either way (Prusa). A temperature tower finds the value for your spool; print speed and acceleration covers speed limits in general.

Good at first, then worse: a partial clog or heat creep

A partial clog lets some plastic through, but not enough. Prusa's early signs: uneven extrusion, much thinner lines, and filament that curls up and sticks to the nozzle when you purge. Bambu Lab separates the hotend from the extruder with a simple test on its A1: take the hotend out, enable maintenance mode, set 170 °C (the lowest extrudable temperature) and extrude. If the extruder feeds freely without the hotend, the hotend is blocked.

If the trouble starts about the same time into every print, whatever the model, suspect heat creep (Teaching Tech). PLA in an enclosure is the classic case: with Prusa's enclosure closed and a room above 27 °C, the inside can get too warm for PLA. Clear the blockage with clearing a clogged nozzle and fix the cause with heat creep explained.

Ground filament or a bite mark: the extruder's grip

The drive gear must grip the filament without crushing it. Too loose and it slips; too tight and it grinds the filament (Prusa). With no filament loaded, the idler screw on an MK3S sits about flush to 1 mm proud of the plastic; on Nextruder printers the screw tips line up with the front of the idler nut. Clean ground plastic out of the gear teeth with a toothpick or the bundled needle.

A trench chewed into the filament usually means the gear slipped against a blockage further down (Teaching Tech). So clear the nozzle first, then clean the gear. On printers with a plastic extruder arm, check the arm for cracks: a cracked arm lets the grip come and go. Chris Riley's under-extrusion video starts with extruder maintenance at 1:01 and replaces printed extruder parts from 3:47.

Under Extrusion - 3D Printer Troubleshooting - Chris's Basement (Chris Riley)

If the extruder also clicks, work through extruder clicking or skipping.

Bubbles, popping or a special filament: the spool itself

Water in the filament turns to steam in the nozzle and causes bubbles, stringing, poor flow and rough surfaces (Bambu Lab). PA, PC and fibre-filled grades are the most sensitive; Prusa adds soluble filament, PETG and ABS. Dry the spool, print the same part again and compare; the signs of wet filament and the drying temperature chart give the details.

Filled filaments need a bigger nozzle. Prusa says wood-filled filament may need at least 0.6 mm; Bambu Lab recommends 0.6 or 0.8 mm for fibre-filled grades and warns against 0.2 mm. After printing a hotter material, load the new filament at the old, higher temperature so it pushes the remains out (Prusa).

Only then: flow, pressure advance and e-steps

When the hardware is sound and small gaps remain, it is a calibration matter. Three settings, three different jobs:

  • Flow (extrusion multiplier, flow ratio) corrects small, even gaps for one filament. Prusa says it is not needed on a new printer from the factory; typical values are 0.9 to 1.1. Bambu Lab advises keeping the default flow ratio for its own filaments. In Bambu Studio it is Calibration → Flow Rate; the method is in flow rate calibration.

  • Pressure advance fixes gaps at corners and where the head speeds up or slows down (Bambu Lab). See pressure advance and linear advance.

  • E-steps or rotation_distance only need attention after a change to the extruder hardware; see calibrating e-steps and rotation_distance.

Calibrate on a clean machine. Bambu Lab warns that a dirty extruder or a partly clogged nozzle skews the result. Factorian Designs shows the flow ratio test in OrcaSlicer in the chapter that starts at 12:58.

Filament Calibration Masterclass – 95% do it wrong! (Factorian Designs)

Common mistakes

  • Raising flow to cover a wrong filament diameter. The 2.85 mm mismatch above would need 265 % flow; set the right diameter instead.

  • Calibrating e-steps through a hot nozzle and then lowering them because the extruder skips. That only asks for less plastic; slowing down or printing hotter fixes the cause (3D Printing Stack Exchange).

  • Blaming the extruder for a first layer that was simply too close. A nozzle scraping the plate causes skipped steps and thin lines that look like under-extrusion everywhere.

When to stop, and where to go next

Some causes are worn or broken parts:

  • A hotend fan blocked by a strand of filament or mounted the wrong way round lets the melt zone creep up (Prusa).

  • Persistent extrusion problems at the correct temperature can mean a worn heater cartridge (Bambu Lab).

  • The extruder motor itself rarely fails. Bambu Lab's test on its X1 and P1: with the extruder removed, a healthy motor gear cannot easily be stopped by hand; wear cut-resistant gloves, because the gear edges are sharp.

  • An old or heavily used nozzle is often better replaced than cleaned (Prusa).

Switch the printer off, unplug it and let the hotend cool before you open the extruder or hotend; Bambu Lab warns that working on a powered toolhead risks a short circuit. If none of the checks helps, contact the printer maker's support with photos and the steps you tried.

The neighbouring guides go deeper on each cause: clearing a clogged nozzle for blockages, extruder clicking or skipping when the motor slips, and flow rate calibration for the last few per cent. If you need the part rather than the practice, the 3D printing service prints PLA and PETG parts from your file.