Filament drying chart: temperatures and times the manufacturers publish
By Sina Esfahani, OmniTechs · Published 22 November 2026
There is no single drying setting per material. For PLA, six published settings from five makers run from 45 to 55 °C and from 4 to 12 hours. For PETG they run from 45 to 65 °C and 4 to 8 hours, and for nylon from 60 to 100 °C and 4 to 12 hours. The setting on the page of your own spool comes first; this chart shows how far the other makers sit from it.
Every row is that maker's recommendation for its own filament or drying device, read on 22 November 2026. OmniTechs did not test these settings.
Published drying settings by material and maker
Filament drying temperatures and times by material and maker
| Material | Source | Drying temperature | Drying time |
|---|---|---|---|
| PLA | Prusa (Prusament PLA) | 45 °C | 6 h |
| PLA | Bambu Lab, AMS HT dryer | 45 °C | 12 h |
| PLA | Bambu Lab, convection oven column | 50 °C | 8 h |
| PLA | Polymaker (PolyLite PLA) | 55 °C | 6 h |
| PLA | eSUN (dryer reference table) | 45 to 50 °C | 4 to 8 h |
| PLA | colorFabb (PLA Economy) | 50 °C | 4 h |
| PETG | Prusa (Prusament PETG) | 55 °C | 6 h |
| PETG | Bambu Lab, AMS HT dryer | 65 °C | 8 h |
| PETG | Bambu Lab, convection oven column | 60 to 65 °C | 8 h |
| PETG | Polymaker (Polymaker PETG) | 60 °C | 6 h |
| PETG | eSUN (dryer reference table) | 45 to 50 °C | 4 to 8 h |
| PETG | colorFabb (PETG Economy) | 65 °C | 6 h |
| ABS | Bambu Lab, AMS HT dryer | 80 °C | 8 h |
| ABS | Bambu Lab, convection oven column | 75 to 85 °C | 8 h |
| ABS | Polymaker (PolyLite ABS) | 70 °C | 6 h |
| ABS | eSUN (dryer reference table) | 60 to 80 °C | 4 to 8 h |
| ASA | Prusa (Prusament ASA) | 80 °C | 4 h |
| ASA | Bambu Lab, AMS HT dryer | 80 °C | 8 h |
| ASA | Bambu Lab, convection oven column | 75 to 85 °C | 8 h |
| ASA | Polymaker (Polymaker ASA) | 70 °C | 7 h |
| ASA | eSUN (dryer reference table) | 50 to 55 °C | 4 to 5 h |
| ASA | colorFabb (ASA) | 60 °C | 6 h |
| TPU | Prusa (Prusament TPU) | 60 °C | 4 to 6 h |
| TPU | Bambu Lab, AMS HT dryer | 75 °C | 18 h |
| TPU | Bambu Lab, convection oven column | 70 °C | 8 h |
| TPU | Polymaker (PolyFlex TPU95) | 70 °C | 8 h |
| TPU | eSUN (dryer reference table) | 50 to 55 °C | 4 to 5 h |
| TPU | colorFabb (TPU 95A) | 75 °C | 6 h |
| Nylon (PA) | Prusa (Prusament PA11 Carbon Fiber) | 90 °C | 6 h |
| Nylon (PA) | Bambu Lab, AMS HT dryer | 85 °C | 12 h |
| Nylon (PA) | Bambu Lab, convection oven column | 75 to 85 °C | 8 to 12 h |
| Nylon (PA) | Polymaker (PolyMide CoPA) | 100 °C | 8 h |
| Nylon (PA) | eSUN (dryer reference table) | 60 to 80 °C | 4 to 8 h |
| Nylon (PA) | colorFabb (PA Neat) | 70 to 80 °C | 4 to 6 h |
Notes on the rows:
Prusa lists settings for its Prusament filaments and has no ABS row. Its separate nylon article says to dry polyamide for at least 4 hours below 90 °C.
Bambu Lab publishes one setting per device. The chart shows its AMS HT dryer and the column it labels "Convection oven". The page does not describe that oven, and this chart reproduces the label only.
Polymaker values are the "Drying setting" on each product's wiki page.
eSUN gives reference ranges adapted from the settings of its eBOX PLUS dryer, groups several materials under one range and says they are not universal settings.
colorFabb values come from its print-support table, except nylon, which comes from the PA Neat product page.
The range per material
Lowest and highest published drying setting per material
| Material | Rows compared | Lowest to highest temperature | Temperature spread | Lowest to highest time |
|---|---|---|---|---|
| PLA | 6 | 45 to 55 °C | 10 °C | 4 to 12 h |
| PETG | 6 | 45 to 65 °C | 20 °C | 4 to 8 h |
| ABS | 4 | 60 to 85 °C | 25 °C | 4 to 8 h |
| ASA | 6 | 50 to 85 °C | 35 °C | 4 to 8 h |
| TPU | 6 | 50 to 75 °C | 25 °C | 4 to 18 h |
| Nylon (PA) | 6 | 60 to 100 °C | 40 °C | 4 to 12 h |
PLA is the material the makers agree on most: 10 °C between the lowest and the highest setting. Nylon and ASA are where they differ most, by 40 °C and 35 °C. The range describes what is published. It is not a window in which any spool of that material is safe.
Why the makers differ
Formulation and grade. eSUN writes that drying needs vary with the manufacturer, the formulation, the filament diameter, the moisture already absorbed and the spool. The nylon rows also cover different grades: Prusa's and Bambu Lab's are fibre-filled.
The device. Bambu Lab says the parameters vary with the drying container. Its AMS 2 Pro stops at 65 °C, and Bambu marks that setting as possibly incomplete for ABS, ASA, TPU and nylon.
The spool. Prusa says its older black spools with a cardboard core stay tight only up to 45 °C. Bambu Lab separates spools rated to 70 °C from spools rated to 90 °C.
Two pages, one maker. eSUN's dryer table gives 45 to 50 °C for PETG; its FAQ gives 60 to 65 °C. colorFabb's product page for PA Neat gives 70 to 80 °C, while its print-support table lists a much higher 125 °C for the same grade. This chart uses the product page.
Signs of wet filament, as the makers describe them
Prusa: poor surface quality first; with a lot of water also weak layer adhesion, blobs, and bubbling and smoke during extrusion.
Bambu Lab: popping sounds from the nozzle, bubbles during extrusion, more stringing, rough surfaces, holes and weaker layer adhesion.
Polymaker: popping or cracking noises while extruding.
UltiMaker: popping sounds and texture changes; transparent nylon may turn milky and black nylon may lose its gloss.
colorFabb, for PA Neat: excessive oozing on travel moves and a rough outer surface.
Stringing and rough surfaces have other causes as well. OmniTechs' guide to diagnosing PETG stringing treats moisture as a possible explanation, not an established cause, until a controlled comparison supports it.
Too hot, too long and the oven question
Prusa warns that above its listed temperatures "the filament will soften and stick together", and tells readers to keep to the listed times to prevent overdrying. Bambu Lab warns that the settings for ABS or PETG can exceed the softening temperature of PLA and TPU, so those spools must leave the dryer first or they may soften and deform. eSUN writes that excessive heat may deform the filament or soften the spool.
A dryer also has a ceiling. Prusa advises checking that a dryer's specification matches the filament. SUNLU, for example, lists 70 °C as the maximum of its FilaDryer S2; four of the six nylon rows lie entirely above that.
This page does not recommend drying filament in a kitchen oven. Prusa, which discusses home ovens on its drying page, warns that their temperature control is imprecise enough to damage filament, PLA above all, and that many cannot be set low enough.
Storage after drying
Prusa: store filament in a closed box or vacuum bag with desiccant, the most moisture-sensitive materials first. It says badly stored polyamide can take up water of up to 10% of the filament's weight.
Bambu Lab: let the spool cool for 5 to 10 minutes after drying, then seal it in a container with working desiccant.
UltiMaker: keep humidity below 20% for most filaments and check it with a hygrometer. It adds that nylon, TPU and PETG can absorb moisture within 24 hours.
Polymaker: print PolyMide CoPA only from a heated dryer.
How to use the chart
Start with your own spool. Look up the maker's page or data sheet for that product; eSUN says the same about its own table.
Compare it with the range. If your planned setting lies outside the published range, recheck the product name and the unit.
Check two limits: the maximum of your dryer and the heat rating of the spool.
Follow the temperature, the time and the device guidance on the page of that exact product. If your dryer or spool cannot reach or withstand that setting, ask the filament maker what to use instead.
Dry different materials separately when their settings differ.
Store the spool sealed with desiccant as soon as it has cooled.
If prints still string after drying, work through diagnosing PETG stringing one variable at a time. Whether nylon suits the part at all is covered in nylon 3D printing, and the choice between PLA, PETG, TPU and nylon in which 3D-printing material fits your part.