Find the right nozzle temperature with a temperature tower

By Sina Esfahani, OmniTechs · Published 27 November 2026

Start with the temperature range the filament maker gives for your exact product, on the spool or in the datasheet. Then print a temperature tower: one small test shape stacked in bands, each band printed 5 °C hotter or cooler than the next. Pick the band with clean bridges, crisp overhangs, little stringing and layers that do not split. If several bands look good, take the middle of them, and the higher end if you print fast (OrcaSlicer).

The label alone is not enough, because the right value depends on your machine. Heater blocks and thermistor positions differ between hotends (Teaching Tech), a thermistor can read a few degrees off, and faster printing needs more heat (accepted answer on the 3D Printing Stack Exchange). The tower measures what your printer needs for that spool.

Fix it in this order:

  1. Look up the maker's range for your exact filament, for example 200 to 220 °C for Prusament PLA.

  2. Dry the filament first; moisture strings and roughens the surface just like too much heat.

  3. Print a tower across that range in 5 °C steps, at the speed, layer height and cooling you will really use.

  4. Read every band for stringing, overhangs and bridges, surface and layer strength.

  5. Choose the middle of the good bands; go higher for speed or strength, lower for looks (OrcaSlicer, CNC Kitchen).

  6. Save the temperature in the filament profile, with the speed and nozzle you tested.

  7. Never test above your hotend's limit; a PTFE-lined hotend has a lower ceiling than an all-metal one.

What too hot and too cold look like

Reading a temperature tower band

Signs from the OrcaSlicer temperature page, Teaching Tech's calibration guide, Prusa's stringing article and Simplify3D's print quality guide, read on 27 November 2026.
What you see on a bandWhat it meansWhat to do
Strings and hairs between the postsUsually too hot (very cold can string too)Go 5 to 10 °C cooler (Prusa, Simplify3D)
Drooping overhangs, sagging bridges, blobby small spikesToo hot for the part coolingGo cooler, or improve cooling
Glossy surface, sometimes with ripplesHotterFine if strings and overhangs are acceptable
Dull surface with sharp detailCoolerFine if the layers still hold
Layers split or the spike snaps along a layer lineToo coldGo about 10 °C hotter (Simplify3D)
Thin, gappy lines, clicking extruder or a jamToo cold for the speedGo hotter or print slower

Weak layers have causes besides temperature: see layer separation. A clicking extruder on the cold bands is covered in extruder clicking or skipping.

Start from the filament maker's range

Each maker publishes a range for its own grade, and the ranges differ even within PLA. Use the one for the product on your spool, not a generic chart.

Published nozzle temperatures for some PLA and PETG grades

Values from the makers' product pages and colorFabb's print support table, read on 27 November 2026. Ranges in brackets are the ± figures written out. Products and values change.
FilamentMaker's nozzle rangeNote from the maker
Prusament PLA210 ± 10 °C (200 to 220 °C)Part cooling fan 100 %
Polymaker PolyLite PLA190 to 230 °CBased on a 0.4 mm nozzle
colorFabb PLA Economy195 to 220 °CFrom colorFabb's print support table
Prusament PETG250 ± 10 °C (240 to 260 °C)Part cooling fan 50 %; PETG tends to ooze
Polymaker PETG240 to 260 °CVery hygroscopic, keep it dry
colorFabb PETG Economy235 to 255 °CFrom colorFabb's print support table

The datasheet tells you more than the temperature; the datasheet comparison for PLA, PETG, ASA and TPU shows how to read the rest.

Stay inside your hotend's limits. Teaching Tech warns that a temperature that is too high can damage parts such as an internal PTFE tube, and your firmware has a maximum it will not exceed. Check the difference between all-metal and PTFE-lined hotends before you test above the usual range.

How to print a temperature tower in your slicer

OrcaSlicer has the most complete built-in tower.

  1. Select the printer and the exact filament profile.

  2. Open Calibration, then Temperature.

  3. Check the range. OrcaSlicer fills in the filament profile's recommended range, rounded to 5 °C steps.

  4. Leave Auto-scale for nozzle on. The tower then scales to your nozzle, with a layer height of half the nozzle diameter.

  5. Print it. The bottom block is the start (hottest) temperature, and each block above is 5 °C cooler.

Worked example: for PolyLite PLA (190 to 230 °C), the tower runs from 230 °C at the bottom to 190 °C at the top, nine blocks in all. With a 0.4 mm nozzle each block is 10 mm tall. A clean block whose lower edge sits at 20 mm is the third from the bottom: 230 − 2 × 5 = 220 °C.

Bambu Studio lists the temperature tower among the calibrations for third-party printer profiles, which need Developer Mode (Preferences, Developer Mode).

PrusaSlicer works with any tower model. Slice it, then in the preview drag the layer slider to the first layer of each band. Right-click the orange plus icon, choose Add custom G-code and enter M104 with that band's temperature, for example M104 S215. Prusa names the temperature tower as a typical use and asks you to verify the codes twice. It needs PrusaSlicer 2.2 or newer and does not work with sequential printing.

Cura does the same with the bundled ChangeAtZ script (marked experimental): Extensions, Post Processing, Modify G-Code. Add one script per band, set the trigger height and tick Change Extruder 1 Temp.

Teaching Tech's calibration site generates a five-band tower with the coolest band at the bottom and the hottest at the top, the opposite of OrcaSlicer. Note which way your tower runs before you read it, and watch the printer while it runs generated G-code.

This video walks through the OrcaSlicer temperature calibration from start to finish.

Orca Slicer Temperature Calibration (The Buildplate Brain)

A tower only answers the question you ask it. Keep everything else as it will be for the real part.

  • Same speed. A fast print has to melt more plastic per second, so it needs a hotter nozzle; slow down, and the same temperature strings and oozes (Bambu Lab's PETG guide). The Stack Exchange answer cited at the top puts the effect of speed at up to about 10 °C. See print speed and acceleration.

  • Same layer height, cooling and nozzle. Print a new tower after you change nozzle size; OrcaSlicer rescales its tower to the nozzle you select.

  • Dry filament. Moisture causes strings and rough surfaces that look like a temperature problem; check the signs of wet filament first.

  • The same spool. Colours of one brand can need different temperatures, the answer adds. Teaching Tech re-tests after a hotend change and for every new brand or type.

Read the tower band by band

Look at each band in the same order:

  1. Stringing between the posts or spikes.

  2. Overhangs and bridges: where do they start to droop?

  3. Surface: gloss rises with temperature, and so can ripples.

  4. Strength: Teaching Tech's tower has a narrow spike in every band to snap off by hand.

Teaching Tech's own PLA example on a direct drive Ender 3 spanned 180 to 260 °C in 20 °C steps. Surfaces got glossier and more rippled as it got hotter, the coolest spike was very brittle and the middle one the strongest. He then considered moving from 200 to 210 °C for more layer strength.

Then choose. A hotter band gives stronger layers and a cooler one sharper overhangs, so the answer depends on the part. OrcaSlicer's middle-of-the-good-range rule is a sound default. Temperature and retraction affect each other (Teaching Tech), so you may tune back and forth with the retraction settings.

Teaching Tech's short clip shows how to read a finished tower.

Interpreting temperature tower results (Teaching Tech)

Looks or strength: what a layer-strength test found

Snapping spikes by hand is rough. Stefan Hermann of CNC Kitchen measured it: he printed standing tensile samples of one PLA and one PETG (both dasFilament) on a Prusa MK3 across their temperature ranges and pulled them apart. Standing samples break between layers, so each result shows how well the layers held.

Layer strength against nozzle temperature in CNC Kitchen's test

Results published by CNC Kitchen for one brand of PLA and PETG on one printer, read on 27 November 2026. Samples printed lying reached about 60 MPa (PLA) and 55 MPa (PETG). Other filaments and printers will differ.
MaterialNozzle temperatureStrength of standing samples
PLA190 °C20 MPa (badly under-extruded)
PLA200 °C37 MPa
PLA210 °C39 MPa
PLA230 °C40 MPa
PLA250 °C37 MPa
PLA270 °C32 MPa
PETG200 °C18 MPa
PETG215 °C22 MPa
PETG230 °C30 MPa
PETG245 °C32 MPa
PETG260 °C24 MPa

His conclusion: print at the lower end of the range for looks, and at the upper end or slightly above for strength. Too hot weakened the layers again, which he suspects comes from moisture and bubbles, and the hottest parts strung badly. Emissions usually rise with temperature as well; see 3D printer fumes and ventilation. The video shows the test, with a chapter on temperature towers near the start.

Stronger 3D prints at higher temperatures? (strength test!) (CNC Kitchen)

When the tower gives no clear answer

  • Every band strings. Dry the filament and check that the nozzle is fitted without leaks (OrcaSlicer). PETG tends to ooze more than PLA (Prusa); the PETG stringing diagnosis tests one cause at a time.

  • Every band is weak. The range may suit another speed, or the problem is cooling, flow or under-extrusion rather than temperature.

  • All bands look the same. Widen the range or, once you know the region, print a second tower with smaller steps inside it.

  • The printer cannot hold the temperature or shows a heating error. Stop testing, switch the printer off and read about the thermal runaway error before you print again.

Save the chosen temperature in the filament profile together with the speed and nozzle you tested at. Then move on to flow rate calibration, which assumes the temperature is set; OrcaSlicer calibrates temperature first because every later test depends on it. If you would rather receive the finished part than tune a spool, the 3D printing service prints PLA and PETG parts from your file.