How to hollow a resin print without suction failures or trapped resin

By Sina Esfahani, OmniTechs · Published 27 November 2026

Hollowing saves resin and weight, and it lowers the force that pulls each layer off the film, because less area cures per layer (Anycubic, Prusa). But a hollow model only prints well when it is open. A closed cavity acts as a suction cup while printing and keeps liquid resin inside afterwards, where it can leak or crack the model later.

So hollow only medium and large models. Start with a 2 mm wall: Prusa advises not going lower, and Elegoo calls 1 to 3 mm a common choice. Then drill at least two drain holes of 3.5 mm or more: one as close to the build plate as possible and one far from it, so resin can flow out and air can flow in (Anycubic, Formlabs). Check a cross-section before you slice. After printing, drain, wash and dry the inside before curing.

Hollow it in this order:

  1. Decide: small models print solid, medium models hollow, large models hollow with an internal lattice or pillars.

  2. Orient the model first, so the face nearest the plate is one you will not see.

  3. Hollow with a 2 mm wall; use high hollowing accuracy for thin walls.

  4. Add two holes of at least 3.5 mm: one beside the plate, one at the far end. Add more wherever the slicer flags a cup.

  5. Check a cross-section: every hole goes through the wall, and no closed pocket remains.

  6. After printing, drain the cavity, wash the inside, let the solvent run out, dry fully, then cure.

Diagnose a failed hollow print

What you see, what it means and what to do

Symptoms and fixes from the Formlabs, Anycubic, Prusa and Elegoo documentation, read 27 November 2026.
What you seeWhat it meansWhat to do
A hole or a large ragged rupture in a wall; resin splashing in the printerA cupping blowout: a cavity acted as a suction cup (Formlabs)Add a drain hole to that cup, reorient, or thicken the wall
The hollow model tore off the plate and lies on the filmSuction onto the film, with no hole near the plate (Anycubic)Put a hole right beside the plate
Resin weeps out, or the model cracks days laterLiquid resin trapped inside; pressure differences over time (Anycubic, Prusa)Two holes at different heights; wash the inside
Thin spots or pinholes in the shellHollowing accuracy too low for the wall (Prusa)Raise accuracy or thicken the wall
A hole stops short of the cavityHole depth too short (Elegoo)Lengthen the hole, or use automatic depth (PreForm)
Thin parts were left solidRegions thinner than twice the wall are not hollowed (PreForm)Normal behaviour; nothing to fix
The model feels fragileThe wall is too thin for its size (Formlabs)Thicker wall, internal lattice or pillars

Should you hollow this model?

Anycubic's rule is "small solid, medium hollow, large structure". Small models print solid. Medium models can be hollowed without filling. Large models need a lattice or other internal structure so they keep their strength. Formlabs adds that a thin shell makes large models fragile, so every millilitre you save costs some strength.

The savings can be large. In Formlabs' own example, hollowing a model with a 2 mm wall on a Form 4 in White Resin V5 saved 177.02 mL of resin, a 77% cut. Formlabs also notes that a hollow part needs fewer supports. If you need the part solid after all, Formlabs suggests filling the shell with epoxy or plaster after printing.

Hollowing is a poor choice where the inside cannot be reached or cleaned. Anycubic names cleaning as the main drawback: a badly cleaned interior can crack the model after it has stood for a long time.

How thick to make the wall

Wall thickness guidance for hollow resin models

As published by Prusa, Elegoo, Formlabs and Mango3D (Lychee Slicer), read 27 November 2026. A slicer's minimum is what the software allows, not a recommendation.
SourceWhat it says
Prusa, PrusaSlicer 2.2 release notesDo not go lower than 2 mm
Prusa, PrusaSlicer hollowing helpThe minimum the tool allows is 1 mm
Elegoo, SatelLite hollowing guide1 to 3 mm is a common choice; thicker walls are stronger
Formlabs, hollowing guideNo range given; its worked example uses 2 mm and warns that thin shells make large models fragile
Formlabs, PreForm hollowingRegions thinner than twice the chosen wall are not hollowed
Lychee Slicer documentationWall thickness can be set from 0.5 to 10 mm

Two settings decide whether the wall you set is the wall you get. A low hollowing accuracy can leave the wall uneven, so Prusa recommends high accuracy for thin shells. PrusaSlicer's closing distance fills small cavities and sharp inner corners where thick resin would otherwise stay behind. When in doubt about wall or hole size, Elegoo suggests a small test print first.

Drain holes: how many, how big and where

Every maker that documents hollowing asks for at least two holes.

Drain hole guidance from the makers

Hole guidance from Anycubic, Formlabs, Prusa and Elegoo, read 27 November 2026. Formlabs warns that holes under 0.5 mm (Form 3) or 0.8 mm (Form 2) may close during printing.
SourceNumber and positionSize
Anycubic, hollow and punch settingsTwo at different heights: one near the plate against suction onto the film, one far from it to equalise pressure and help cleaningNot stated
Formlabs, hollowing guideOne as close to the build platform as possible, at least one more, and more where PreForm flags a cupSet in PreForm
Formlabs, design specificationsFor any fully enclosed cavityAt least 2.5 mm diameter (Form 3); 3.5 mm (Form 2)
Prusa, PrusaSlicerAt least two, ideally on opposite sides; more is betterConfigurable
Elegoo, SatelLiteAt the lowest point of the hollow area, plus at least one more so solvent can flow in and outRadius about 1 to 3 mm, so 2 to 6 mm across

A 3.5 mm hole meets both Formlabs minimums and sits inside Elegoo's range, which makes it a sensible default. Three details decide whether the holes work:

  • "Lowest point" means closest to the plate. In the slicer view the plate sits at the bottom, so Elegoo's lowest point and Anycubic's "near the platform" are the same place.

  • The hole must go through the wall. Elegoo warns that a short hole may not reach the cavity. PreForm's Automatic Depth Mode finds the depth for a through-hole, and Lychee marks holes it cannot drill in red.

  • Hide them. Put the holes on a face nobody sees, so they do not spoil the look (Formlabs, Prusa). Elegoo SatelLite's Keep Hole Pin option also prints a matching plug to close a hole afterwards.

Why a closed cavity fails: suction cups and blowouts

Formlabs explains cupping as a problem of upside-down resin printing. A hollow or concave area traps air or resin like a suction cup. As the plate rises and the layer peels, the space inside grows and the pressure drops, pulling the walls of the cup inwards. Thin walls buckle. The result is a hole in the wall, a ragged rupture, a poor surface on the cup, or resin splashing when the cup lets go. Small cups and thick walls may print fine; the risk depends on the resin, the cup size, the shape and the wall.

An accepted answer on the 3D Printing Stack Exchange compares it with lifting a bottle out of a liquid upside down: nothing drains until its rim leaves the surface or a wall gives way, and the release can be violent enough to deform the print. For an open shape such as a cup, the answer suggests printing it on its side so resin and air can flow freely.

Formlabs' fixes are a drain hole in the cup and a different orientation; PreForm can highlight cups before you print. Its short video shows the symptoms and the cup detection, with a chapter for each step.

How To Prevent Suction Cups and Blowouts in PreForm | Formlabs (Formlabs Support)

Orientation and hollowing work together. Formlabs warns against orientations with several negative overhangs, which trap resin as well; general orientation trade-offs are in choosing a 3D print orientation. The same suction is a common reason for a resin print not sticking to the build plate.

Where to find hollowing in your slicer

Hollowing, holes and checks in four resin slicers

Menu names from the Prusa, Mango3D, Elegoo and Formlabs documentation, read 27 November 2026. Menus move between versions; PreForm hollowing needs version 3.41.0 or later.
SlicerHollowingDrain holesHow to check the result
PrusaSlicerHollowing tool in the left toolbar, or Print Settings, Hollowing: thickness, accuracy, closing distanceLeft-click the model with the hollowing tool open; holes are always perpendicular to the surfacePreview hollowed and drilled model, then the clipping plane
Lychee SlicerPrepare, Hollow, Hollowing 3D, or Voxel Hollowing 3D with Detect pocketsHoles drill through to the cavity; red holes are ignoredLayer preview slider; yellow voxels show filled traps
Elegoo SatelLiteHollow in the top menu: thickness, precision, hollowing type, then ConfirmHoles in the top menu: outer and inner radius, length long enough to pierce the wallInspect the hollowed model before slicing
Formlabs PreFormHollow in the left toolbar: wall thickness, then Hollow SelectedHole tool: radius, padding, depth or Automatic Depth ModeCups toggle in the Print Validation menu

Two cautions. PrusaSlicer shows the model unhollowed and undrilled again after you change a parameter, move a hole or scale the model, until the hollowing is recalculated, so check the preview after every change. PreForm hollows a model made of several separate pieces piece by piece, which can give unexpected results. If your slicer leaves islands inside, as one Chitubox user reported on the Stack Exchange, the answer there pointed to Lychee Slicer or PrusaSlicer.

Lychee's own tutorial below walks through a full hollowing, with chapters on whether to hollow at all, holes and suction cups, internal supports and the different hole types.

How to Hollow Your 3D Model? | Lychee Slicer Tutorial (Lychee)

Worked example: a 12 cm bust

Say you print a 12 cm bust upright on supports, base towards the plate.

  1. It is medium-sized, so hollow it without filling (Anycubic).

  2. Set a 2 mm wall with high accuracy (Prusa).

  3. Drill hole one, 3.5 mm, in the underside of the base, right beside the plate; it is hidden once the bust stands.

  4. Drill hole two, 3.5 mm, at the far end of the cavity, for example at the back of the head under the hair line, to let air in and help washing.

  5. Run the slicer's cup check and look at a cross-section. A closed pocket under the chin, say, gets a third hole.

  6. Compare the resin volume before and after hollowing; Formlabs' example with a 2 mm wall saved 77%, but your model will differ.

Clean and cure the inside

Liquid resin left inside stays liquid. Prusa warns it is likely to leak out if the object ever breaks, and Anycubic links a poorly cleaned interior to cracking later. So clean the inside as carefully as the outside.

  1. Drain the cavity through the holes as soon as the print comes off; leftover resin uses up the wash liquid faster (Anycubic).

  2. When washing by hand, fill the cavity with solvent and shake it through (Anycubic). In a wash station, let the solvent run out into the bucket before you lift the part away (Formlabs).

  3. Flush narrow channels with a syringe of clean solvent; they may not drain on their own (Formlabs).

  4. Dry the part fully, inside too, before curing.

  5. Cure as usual. Light only reaches what it can see, so the wash, not extra curing time, is what makes the inside safe.

Handle a cracked or broken hollow print with gloves: the resin that leaks out is still a liquid sensitiser (resin printer safety at home). Wash and cure times are in washing and curing resin prints.

When not to hollow, and when to stop

  • Functional, load-bearing parts. A shell is weaker than a solid; Formlabs warns that thin shells make large models fragile.

  • Thin models. Areas thinner than twice the wall are not hollowed anyway (PreForm), so hollowing gains little.

  • Cavities you cannot reach with holes. If a pocket cannot be drained, fill it (PrusaSlicer's closing distance, Lychee's pocket detection) or print solid.

  • A hollow print that leaks after curing. Do not seal the holes over it. Drain, wash and cure it again, or cure it and dispose of it as resin waste.

To judge the finished result on a display piece, see assessing resin for small display details. OmniTechs does not print resin; the comparison of FDM, SLA and SLS helps you decide whether a filament print would suit the part instead.