How to print TPU: start settings by hardness and extruder, and fixes for jams and stringing
By Sina Esfahani, OmniTechs · Published 27 November 2026
Print TPU slowly, with a gentle extruder and a dry spool. Start from your slicer's TPU profile; if there is none, cap the flow at 2 mm³/s, about 22 mm/s on a 0.4 mm nozzle at 0.2 mm layers, and raise it in small steps. Loosen the extruder idler.
How soft the TPU is decides whether your printer can feed it at all. 95A prints on most printers, slowly on a Bowden; 90A needs direct drive; 85A needs dedicated hardware. And standard TPU does not go through an automatic multi-material unit: Bambu Lab's AMS feeds only its much stiffer TPU for AMS.
Get the first print through in this order:
Match the hardness to your extruder: 95A on most printers (slowly on Bowden), 90A on direct drive only, 85A on dedicated hardware.
Dry the spool: 70 °C for 8 hours (Bambu Lab TPU 95A HF, Polymaker PolyFlex TPU95).
Fit a clean nozzle of 0.4 mm or larger and loosen the idler.
Start from the slicer's TPU profile, or cap the flow at 2 mm³/s.
Keep the profile's retraction and change it in 0.2 mm steps: more against oozing, less against holes in the surface.
Keep the fan off for the first layer, then follow the profile; turn it down if layers split.
Feed from a free-running spool holder or a dry box, not through an automatic multi-material unit.
What you see and what to do
TPU problems, what they mean and what to do
| What you see | What it means | What to do |
|---|---|---|
| Filament bunches up or escapes beside the drive gear | It buckles between the gear and the hotend | Print slower, loosen the idler, close the gap in the path, or use a harder grade |
| Extruder clicks, thin or missing lines | More flow than the hotend can melt, or too much feed resistance | Lower the flow cap; feed from a free-running spool; dry the filament |
| Strings and hairs between parts | Wet filament, oozing pressure or long travel moves | Dry it; add 0.2 mm retraction; print one object at a time; check the start G-code |
| Small holes or pits in the surface | Wet filament or too much retraction | Dry it; remove 0.2 mm retraction |
| Overhangs droop, thin sloped walls wobble | Soft walls, or a worn nozzle | More walls; check the nozzle opening; a little more fan |
| The print is welded to the plate | TPU bonds very strongly | Glue stick or tape as a separator; alcohol into the gap to lift it |
| Jams inside a warm enclosure | TPU softens in the extruder | Open the door or top; do not heat the chamber |
Shore hardness: what your printer can feed
TPU hardness is given on the Shore scale, measured by pressing a pin into the material. A lower number is softer; the letter is the scale, D for harder grades and A for the softer ones most TPU filaments use. Bambu Lab's order from hard to soft: 77D, 70D, 68D, 55D, 95A, 90A, 85A, 83A, 80A, 75A, 70A.
For printing, the number is a difficulty rating, because soft filament buckles and tangles in the extruder gears:
95A and harder print on most printers if you go slowly. High-flow grades such as Bambu Lab's TPU 95A HF and Polymaker's PolyFlex TPU95-HF, which Polymaker places closer to 98A, are made to run faster.
90A needs a direct-drive extruder according to Polymaker, which expects extrusion problems on a Bowden setup.
85A and softer need dedicated hardware. Bambu Lab does not support its TPU 85A on the A1 series, and allows it only on standard nozzles of 0.6 mm or larger or on its TPU high-flow hotend.
Polymaker adds that hardness is only an indication of how soft the part will be: walls, infill, top and bottom layers and layer height change the feel as much as the grade does.
Extruder and filament path
TPU fails when it can bend sideways between the drive gear and the hotend. That is why the makers prefer direct drive, and why Polymaker says the longer the path to the hotend, the slower you must print. Any open gap between the drive gear and the hotend inlet is where it folds out.
Bowden printers can still print the harder grades. UltiMaker's own Cura profile for TPU 95A on its S5, a Bowden printer, prints at 25 mm/s with an 8 mm retraction.
Before the first print:
Loosen the idler. Prusa tells you to set the idler looser than normal for TPU, so the gears push gently and do not squash the filament.
Start with a clean nozzle. Bambu Lab recommends a new nozzle or a cold pull, and not reusing a nozzle that printed carbon- or glass-fibre filament, because leftover fibres raise the resistance; see clear a clogged nozzle with a cold pull.
Use the maker's flex path. Prusa's CORE One+ and CORE One L have a latch that loosens the filament sensor lever for flexible filament, and its XL needs a printed bypass because of its long filament path. Bambu Lab offers a TPU feeding assist module for its H2, X and P series.
Start settings from the slicer profiles
Start values for TPU in slicer profiles and on filament makers' pages
| Source | Nozzle (°C) | Flow cap or speed | Part cooling fan | Retraction |
|---|---|---|---|---|
| Bambu Studio, Generic TPU | 240 | 3.2 mm³/s | 100%, off for the first layer | 0.4 mm |
| Bambu Studio, Bambu TPU 95A HF on the X1C and A1 | 230 | 12 mm³/s | 100%, off for the first layer | 0.8 mm |
| PrusaSlicer, Generic FLEX for older extruders such as the MK3 | 240 | 1.2 mm³/s | off; 80% on bridges | 0 mm |
| PrusaSlicer, Generic FLEX for the MK4 | 230 | 3 mm³/s | 30 to 60% | 2.5 mm |
| Cura, UltiMaker TPU 95A on the S5 with an AA 0.4 core | 225 | 25 mm/s print speed | 20% | 8 mm |
| Polymaker PolyFlex TPU95, product page | 210 to 230 | 30 to 50 mm/s | on | 3 to 6 mm |
The makers disagree on fan and retraction, and the extruder explains most of it. Prusa's flexible-materials guide says print cooling off and retraction low or off, and its profile for older extruders does exactly that. Its current profile for the MK4 runs the fan at 30 to 60% and retracts 2.5 mm. A Bowden printer like UltiMaker's needs a long retraction. Start with the values for your type of extruder.
Where to set them:
Flow cap: in Bambu Studio and OrcaSlicer, edit the filament preset, Filament tab, Max volumetric speed. In PrusaSlicer, Filament Settings > Advanced > Max volumetric speed.
Fan: the Cooling tab of the filament preset in Bambu Studio and OrcaSlicer; Filament Settings > Cooling in PrusaSlicer.
Cura keeps its flow-rate limit disabled in the standard definitions, so set Speed > Print Speed, Travel > Retraction Distance and Cooling > Fan Speed directly.
Worked example: from flow cap to print speed
The flow cap (maximum volumetric speed) is the most plastic the hotend may melt per second. Bambu Lab's formula: flow = layer height × line width × speed. With 0.2 mm layers and 0.45 mm lines, each mm/s of speed is 0.09 mm³/s of flow.
PrusaSlicer's 1.2 mm³/s: 1.2 ÷ 0.09 = 13 mm/s.
Prusa's Flexfill 98A profile of 1.5 mm³/s: about 17 mm/s, the figure Prusa itself gives.
Bambu Studio's Generic TPU at 3.2 mm³/s: about 36 mm/s.
TPU 95A HF at 12 mm³/s: about 133 mm/s, only with a high-flow grade and a capable extruder.
No profile for your printer? Prusa's typical range for TPU is 2 to 5 mm³/s. Start at 2 mm³/s, about 22 mm/s, and raise it in small steps. Stop raising when the extruder clicks, lines thin out or layers bond poorly: those are Prusa's signs that the cap is too high.
CNC Kitchen's video on flexible filaments covers drying, tuning the profile and preparing the bed; the start time is the chapter on how to print them.
Stringing, holes and oozing
Some stringing comes with TPU: Prusa calls it inevitable with small retractions, and Polymaker says it is hard to remove every hair. The fixes in the table above work in this order: dry the filament, change retraction in 0.2 mm steps, and print one object at a time to cut travel moves (Bambu Lab).
One cause is easy to miss. On Stack Exchange, a user traced heavy stringing to a start script that over-primed the nozzle: the soft filament compressed in the Bowden tube and oozed for many layers. Reducing the prime fixed it. Retraction in general is covered in retraction settings for Bowden and direct drive.
Drying and storage
Bambu Lab calls TPU highly hygroscopic, lists 1.08% water absorption for TPU 95A HF at 55% humidity, and recommends storage below 20% relative humidity with desiccant. Its drying values for TPU 95A HF are 70 °C for 8 hours in a forced-air oven, or 80 to 90 °C for 12 hours on an X1 heatbed. Polymaker gives 70 °C for 8 hours for PolyFlex TPU95.
Bambu Lab adds that its AMS 2 Pro dries at most at 65 °C, below what TPU needs, and that a spool can swell slightly while drying. Prusa is the exception for its own grade: Prusament TPU 95A absorbs little moisture and needs no drying on its Nextruder printers.
See the filament drying chart for other grades and signs of wet filament to recognise the problem.
TPU in an AMS, MMU or other multi-material unit
Bambu Lab's own compatibility table shows which of its TPUs each feeding route can take.
Which Bambu Lab TPU can use which feeding route
| Feeding route | TPU for AMS (68D) | TPU 95A HF, 90A and 85A |
|---|---|---|
| Automatic feeding in the AMS, AMS lite or AMS 2 Pro | yes | no |
| Automatic feeding in the AMS HT | yes | no |
| AMS HT used as a sealed box, through its TPU outlet | yes | yes |
| AMS 3H or 3P bypass port | yes | yes |
| External spool holder of the AMS 3H or 3P | yes | possible, not recommended |
TPU for AMS is a different material in practice. Bambu Lab's sheets list a tensile modulus of 1,190 MPa for it against 9.8 MPa for TPU 95A HF, and an elongation between layers of 31% against more than 480%. It feeds through the AMS because it is much stiffer. Other makers are more cautious: Polymaker suggests avoiding TPU in the AMS, and Prusa warns that automatic filament change may not work properly with flexible filaments.
CreativeMaker's guide to flexible filaments on Bambu Lab printers compares the grades; the start time is the chapter on TPU for AMS.
Supports are a related problem. TPU bonds so well to itself that same-material supports are very hard to remove, according to Polymaker. Bambu Lab recommends PLA as the support material for TPU, and spraying alcohol into the gap to separate them. When TPU supports itself, Prusa suggests a support Z distance of about 0.3 mm and an XY separation of at least 100%.
When to stop and choose another way
Bowden printer, 90A or softer. The makers' own guidance says it will fight you. Use a harder grade, a direct-drive conversion, or have the part printed.
Overhangs fail no matter what you tune. On Stack Exchange, a user chasing TPU overhang failures finally found a worn nozzle whose opening had grown; a new nozzle and a recalibrated pressure advance fixed it. Replace the nozzle before you tune further.
It still tangles at 2 mm³/s with the idler loose. The path is too long or open for that hardness: use a harder grade or the maker's flex path.
Next step and related guides
Which hardness your part needs is a separate question, covered in rubber-like behaviour or a specific TPU grade; check the feel with a small test piece first. The trade-off between extruder types is in Bowden or direct drive extruder.
If you need the part rather than the practice, OmniTechs prints TPU parts after a feasibility check and states the hardness of its filament, with the datasheet, in the quote.
Sources
Bambu Lab Wiki: Volumetric speed and how it impacts 3D printing
Bambu Studio on GitHub: Bambu TPU 95A HF profile for the X1C
UltiMaker: Cura quality profile for TPU on the S5 with AA 0.4
UltiMaker: Ultimaker S5 fine knurl feeder kit, installation guide (Bowden tubes)
3D Printing Stack Exchange: Avoiding stringing with flexible filament
3D Printing Stack Exchange: Root cause fix for TPU overhang failures
CNC Kitchen video: Why aren't more people 3D Printing this Indestructable Filament?
CreativeMaker video: Mastering Flexible Filaments on Bambu Lab - the Ultimate Guide