LW-PLA settings: how hot to print, how far to cut the flow, and how to tame the strings
By Sina Esfahani, OmniTechs · Published 27 November 2026
LW-PLA comes in two kinds, and the settings are opposite. Active-foaming grades (colorFabb LW-PLA, eSun eLW-PLA, Bambu Lab PLA Aero) contain a blowing agent that foams in the hot nozzle: the hotter you print, the lighter the part. Pre-foamed PolyLite LW-PLA from Polymaker is foamed in the factory and prints much like normal PLA.
For an active grade, start at 245 °C with a flow ratio of 0.6, Bambu Lab's defaults for PLA Aero, and fine-tune with a single-wall test. Expect oozing on every travel move; retraction barely stops it, so slice for one continuous path. Foaming costs strength faster than it saves weight, so keep it for light skins, RC planes and props.
Set it up in this order:
Check which kind you have: active foaming (colorFabb, eSun, Bambu Lab PLA Aero) or pre-foamed (Polymaker PolyLite LW-PLA).
Active grade: nozzle 245 °C and flow ratio 0.6 (Bambu Lab). Pre-foamed grade: about 190 °C and normal flow (Polymaker).
Part-cooling fan at 30% or lower, and about 50 mm/s for the first layer and outer walls (Bambu Lab).
Print a single-wall test, measure the wall with calipers and lower the flow until it matches the line width you set.
Keep retraction short (1 to 2 mm on direct drive, 3 to 6 mm on Bowden, colorFabb) or switch it off with z-hop, and remove travel moves where you can.
On a Bambu Lab printer, untick Flow Dynamics calibration before you send the print.
Dry the spool (Polymaker: 55 °C for 6 hours) and feed it from a spool holder rather than a multi-material unit.
Read the print: what you see and what to change
LW-PLA problems, causes and fixes
| What you see | What it means | What to do |
|---|---|---|
| Walls too thick, blobs, nozzle clogs | Flow set too high for the foaming | Lower the flow; Prusa's range runs from 1 down to 0.35 and warns that too high may clog |
| Gaps, thin or weak walls | Too little flow or too little foaming for the speed | Raise the flow, or the nozzle by 5 to 10 °C, or slow down |
| Part heavier than planned, colour dark and glossy | The plastic is not foaming fully | Raise the temperature; fully foamed LW-PLA turns lighter in colour (colorFabb) |
| Rough surface, lost detail | Over-foaming | Lower the nozzle in 5 °C steps (colorFabb) |
| Strings and blobs across the part | Ooze on travel moves, normal for active LW-PLA | Fewer travel moves, short retraction, coasting and wiping; trim the rest |
| Loops or ridges at each seam | Retraction and z-hop at the seam | Retraction length 0, which also stops z-hop |
| Popping or crackling at the nozzle | Wet filament | Dry the spool before changing anything else |
| Feed failures in an AMS | LW-PLA is weaker than standard PLA on the spool | Feed from the spool holder at the back (Bambu Lab) |
Active or pre-foamed: check which you have, then start from the maker's values
Bambu Lab's RC guide sorts foaming PLA into two groups. Active-foaming filament expands in the nozzle, so its density depends on temperature, speed and flow. Pre-foamed filament is expanded during manufacture. It is lighter than normal PLA but not as light as a fully foamed active grade, and it hardly reacts to temperature.
That changes every setting. Polymaker says its pre-foamed grade needs no changes from regular PLA apart from slightly more retraction, and prints best at low temperature, around 190 °C. Bambu Lab's RC guide keeps the flow ratio near 1 for pre-foamed grades and around 0.5 to 0.6 for active ones. It suggests about 230 °C for pre-foamed grades in general; for PolyLite LW-PLA, Polymaker's own figure comes first. Settings copied from the wrong kind either over-extrude badly or leave gaps.
Published LW-PLA settings per maker
| Maker and grade | Type | Nozzle | Foaming | Flow | Fan and speed |
|---|---|---|---|---|---|
| colorFabb LW-PLA, product page | Active | 195 to 260 °C | Starts around 230 °C; volume up to nearly three times; parts up to 65% lighter | Three times lower material multiplier when fully foamed | Speed 40 to 100 mm/s; bed 50 to 60 °C |
| colorFabb, LW-PLA tutorial | Active | 210 to 260 °C | Little at 210 to 220 °C, strong at 250 °C and above; volume up to 250% | Cut flow by 20 to 50% at high foaming temperatures | Fan 0 to 50%; 30 to 60 mm/s, best at 30 to 40 mm/s |
| Prusa knowledge base, LW PLA | Active | 210 to 250 °C | Expands 2.3 to 3 times; maximum around 240 to 250 °C | Extrusion multiplier 1 down to 0.35 | Bed 55 to 60 °C on smooth PEI |
| Bambu Lab PLA Aero, RC guide | Active | 245 °C default | Hotter means more foaming | Flow ratio 0.6 default | Fan 30% or lower; about 50 mm/s |
| Polymaker PolyLite LW-PLA | Pre-foamed | 190 to 210 °C | Foamed in the factory | As for normal PLA | Fan on; 50 mm/s for the least stringing |
The figures do not line up exactly. A threefold volume increase implies a flow near a third, yet colorFabb's tutorial suggests a 20 to 50% cut. Prusa explains why: foaming depends on nozzle temperature and print speed together, and faster printing needs more heat for the same expansion. Your printer, speed and line width decide where you land.
Calibrate temperature and flow together
Because the right flow depends on how much the line foams, set both at once. CNC Kitchen's method for colorFabb LW-PLA works on any printer:
Print a simple single-wall part while stepping the nozzle temperature in 5 or 10 °C steps. In CNC Kitchen's test, foaming became visible at 215 °C and peaked at around 240 to 250 °C.
At the temperature you want, print single walls and measure their thickness with calipers.
Lower the flow until the wall matches the line width in your slicer. Then repeat once: expansion also changes with speed and flow.
A worked example of step 3: you set 0.45 mm lines, print at flow 1.0, and the wall measures 0.90 mm. The new flow is 1.0 × 0.45 ÷ 0.90 = 0.50. Print again at 0.50 and measure, because less flow also means slightly different foaming.
The usual tools only help in part. A temperature tower shows where foaming starts but says nothing about flow. The general flow calibration methods assume a material that does not expand. On Bambu Lab printers, untick Flow Dynamics calibration before printing PLA Aero: Bambu Lab says it may not find an accurate value for foaming PLA, and the calibration line itself risks stringing and oozing. Users in the Bambu Lab forum disagree on this point, but if the calibration line strings, untick it.
Stringing and oozing: design around travel moves
colorFabb calls oozing on travel moves normal for LW-PLA and says it cannot be removed completely. Prusa explains why: the material keeps expanding in the nozzle, so retractions do little. Its advice is to print in one pass, such as vase mode, and to avoid moves across empty space. Trim ooze marks with a knife and smooth them with a sanding sponge.
Within those limits:
Remove travel. Check the sliced preview for travel lines across the model before you print (Bambu Lab).
Keep retraction short. colorFabb suggests 3 to 6 mm on Bowden printers and 1 to 2 mm on direct drive. CNC Kitchen's nozzle clogged with more than about 2.5 mm on a Prusa i3 MK3S.
Use coasting and wiping. Polymaker recommends about 0.5 mm of coasting and 1 mm of wiping for its LW-PLA and says this helps most.
Trade weight for cleanliness. A slightly lower temperature strings less (colorFabb).
Seams are a special case. In part three of a widely read Bambu Lab forum series on LW-PLA, the author found that each seam forced a retraction and a spiral z-hop, which left loops and ridges. In Bambu Studio he set Filament Settings, Setting Overrides, Retraction Length to 0, which also disables z-hop on retraction. For the general theory, see the guide to retraction settings for Bowden and direct drive.
How much strength foaming costs
CNC Kitchen tested colorFabb LW-PLA printed at three temperatures. The results show why maximum foaming suits light skins and props rather than load-bearing parts.
CNC Kitchen test of colorFabb LW-PLA at three nozzle temperatures
| Nozzle temperature | Density compared with PLA | Tensile strength | Layer adhesion | Bending stiffness |
|---|---|---|---|---|
| 205 °C, unfoamed | 100% | 49 MPa | About two thirds of the flat strength | 3,200 MPa |
| 225 °C | 67% | 24 MPa | 13 MPa | 1,600 MPa |
| 250 °C | 44% | 12 MPa | 4.3 MPa | 900 MPa |
At 44% of the density, the part keeps only a quarter of the tensile strength and under a third of the stiffness. Impact behaved differently: the samples printed standing up absorbed roughly the same energy at every foaming level, while the flat samples lost impact strength like the other tests. colorFabb's own advice matches: for load-bearing parts, use standard PLA or PETG. CNC Kitchen's video walks through the temperature test, the flow correction and the mechanical tests.
RC planes and props
Settings for RC planes
RC aircraft are the classic LW-PLA use, and the models are designed around the material: single-wall skins and internal ribs that each layer prints as one closed loop, without travel. Follow the model designer's profile first; it is tuned for that airframe. 3DLabPrint publishes its own config bundle, and Prusa supplies one with the even-odd slicing mode for 3DLabPrint planes.
In Bambu Studio, Bambu Lab's RC guide sets:
Precision, Slicing gap closing radius: 0. Others, Special mode, Slicing mode: Even-odd. Both keep the internal structure the designer drew.
First layer and outer wall at about 50 mm/s, with Slowdown for overhangs switched off for an even speed.
First layer 10 °C hotter than the rest; line width above 0.4 mm and layers of 0.15 to 0.25 mm, or as the designer specifies.
For models that suit spiral vase: one wall loop, no top or bottom shells, 0% infill and the Classic wall generator; print several models one by one.
For other models: retraction reduced or off, z-hop off and the seam usually on Nearest.
For Cura, Troy McMillan's RC channel goes through every Cura setting he uses for LW-PLA and compares colorFabb LW-PLA with eSun eLW-PLA.
Cosplay and props
For props and wearables the appeal is weight and finish. colorFabb says LW-PLA is easy to cut, trim and sand, takes paint well and hides layer lines; Prusa adds that it glues easily with CA glue. The guide to sanding, priming and painting PLA applies, with a lighter hand because the foamed surface is softer.
Mind the heat. colorFabb gives a glass transition temperature of 55 °C for LW-PLA, and Prusa lists a lower glass transition temperature among its drawbacks. A helmet left in a hot car or a wing in summer sun can soften; colorFabb sells LW-PLA-HT for that reason. The guide to PLA in a hot car explains the limits.
Storage, drying and feeding
Dry the spool before printing. For prints longer than four hours, Bambu Lab keeps PLA Aero in an airtight container with desiccant while it feeds. Polymaker dries its LW-PLA at 55 °C for 6 hours and says cracking or popping noises mean it needs drying. Figures for other brands are in the filament drying chart.
LW-PLA is weaker than standard PLA on the spool too. Bambu Lab reports occasional feed failures and gear slip in the AMS and recommends feeding PLA Aero from the spool holder at the back of the printer.
When to stop
The nozzle clogs after you raised retraction. Go back below about 2.5 mm, the point where CNC Kitchen's nozzle clogged, and fight strings with travel and coasting instead.
The part has to carry load. No setting gives foamed PLA its strength back; print that part in standard PLA or PETG.
The part will see more than about 55 °C. Choose a heat-resistant grade such as LW-PLA-HT, or another material.
A model will not slice cleanly in vase or even-odd mode. Some early RC models were not designed for it; Bambu Lab suggests slicing them with default settings and printing them in normal PLA.
Next step and related guides
Before a full airframe, spend one evening on the single-wall test, then print a test section of the model with the settings you found; that saves more filament than any profile. OmniTechs does not print foaming filaments; if a light part in standard PLA would do, a print with thin walls and low infill from the 3D printing service may be worth comparing.