Acetone smoothing ABS and ASA: the safe cold method, and what it does to your part
By Sina Esfahani, OmniTechs · Published 27 November 2026
Acetone vapour softens the skin of an ABS or ASA print so the layer lines flow together into a glossy surface. Prusa calls ABS and ASA with acetone by far the most suitable combination for chemical smoothing. It does not work on PLA, and PETG needs a far more dangerous solvent.
The gloss costs shape. Edges round, small text and detail blur, and thin or flat parts can twist, so functional parts are not suitable.
Acetone is highly flammable, with a flash point of about −20 °C: its vapour can ignite at any room temperature. Use only the cold method: paper towels wetted with acetone in a glass or polypropylene box with a loose lid, outdoors or by an open window, never heated and never near a spark.
Do it in this order:
Check the material: ABS or ASA only. PLA will not smooth, and PETG is unreliable.
Check the part: no fits, threads, snap-fits, small text or thin, flat walls.
Work outdoors or by an open window, away from heat, flames, sparks and electrical devices; switch off and unplug the printer if it is in the same room.
Wear safety glasses and gloves rated for acetone, and keep a CO2 or powder extinguisher to hand.
Use a glass or polypropylene box with a loose lid, the part on a raised platform, paper towels wetted without a pool, and the bottle closed and out of the room.
Watch through the side, take the part out as soon as it turns glossy, and never leave it unattended.
Let the part harden for at least several hours, ideally a day; air the box outdoors and take leftover acetone to chemical waste collection.
Is acetone smoothing right for your part?
Choosing a finish by material and part
| Your part | Acetone vapour? | Better route if not |
|---|---|---|
| ABS or ASA display piece, figure or cover | Yes, with the cold method | Not needed |
| ABS or ASA part with fits, threads, snap-fits or sharp edges that matter | No: it changes dimensions and rounds edges | Sanding or a primer, where you control how much comes off |
| Thin or large flat ABS or ASA part | Risky: thin parts twist and flat parts deform | Sanding and primer |
| PLA | No: hours of vapour barely soften it | Sanding and filler primer, or an epoxy coating |
| PETG | No: Prusa smooths it with dichloromethane, a dangerous solvent | Sanding and primer |
| PVB, such as Polymaker PolySmooth | No acetone: it smooths with alcohol | Polymaker's Polysher; alcohol is flammable too |
Results also differ between brands of the same material. In Prusa's comparison of ten ABS and ASA filaments, Prusament ASA was glossy after 15 to 20 minutes in Prusa's warmed box and most others after 20 to 40 minutes, but two still showed layers after an hour. Pigment can also fool you: on one grey ASA, Prusa found the surface mirror-smooth while the layers still showed through the colour.
What it does to detail, dimensions and strength
Smoothing dissolves the surface, so it always changes the shape; as a Stack Exchange answer puts it, the only question is whether the change stays within your tolerance. Prusa lists what to expect:
Small, complex features lose their detail or deform. Forum users report gear teeth coming out with rounded tips.
Large flat parts deform, and thin parts twist and can become unusable.
Sharp edges round off and dimensions change, which is why Prusa rules out functional parts.
The part stays soft for hours. Prusa leaves parts to recover for at least several hours or a whole day, and they can smell of acetone for days.
Lower layer heights smooth better, because there is less ridge to dissolve. The layer height guide explains the trade-off with print time.
Worked example: measure the change before you trust it. No maker publishes how much the vapour takes off. Say your ABS case has a 10.0 mm hole for a pin. Print a small test piece with the same hole and the same layer height, measure it with callipers, smooth it exactly as you will smooth the real part, and measure again after a day. If the hole has closed to 9.8 mm, you now know to design it 0.2 mm larger, or to mask it. The tolerances and clearance guide shows what to measure.
On strength, Prusa's results are mixed: smoothed Prusament ASA had slightly better toughness and more than twice the layer adhesion, but tore at a slightly lower force. The same article calls smoothing purely aesthetic. Do not count on it to make a part stronger.
CNC Kitchen printed test samples, smoothed half of them and compared their strength, with acetone on ABS and alcohol on PolySmooth. Watch it for the test results, not as a method: this guide sticks to the unheated method.
Fire and health: what the safety data sheet says
Read the safety data sheet (SDS) of the acetone you actually bought before you start. A supplier SDS from Fisher Scientific and the international chemical safety card from the ILO and WHO agree on the hazards and differ slightly on the numbers.
Acetone fire data from two safety documents
| Property | Fisher Scientific SDS (revised 18 December 2025) | ILO/WHO safety card ICSC 0087 (April 2024) |
|---|---|---|
| Classification | Highly flammable liquid and vapour | Highly flammable; vapour/air mixtures are explosive |
| Flash point (closed cup) | −20 °C | −18 °C |
| Explosive range in air | 2.5 to 12.8 % by volume | 2.2 to 13 % by volume |
| Auto-ignition temperature | 465 °C | 465 °C |
| Vapour | May travel to an ignition source and flash back | Heavier than air, may travel along the ground; distant ignition possible |
| Extinguishing | Water spray, CO2, dry chemical, alcohol-resistant foam; water may be ineffective | Powder, alcohol-resistant foam, water, carbon dioxide |
What that means in practice:
Never heat acetone. Not on a stove, a hot plate, a rice cooker or the printer's heated bed, even though forum answers describe all of these. The SDS says to keep it away from heat, hot surfaces, sparks and open flames. The safety card warns that heating raises the pressure with a risk of bursting. Prusa itself calls warming acetone dangerous and names paper soaked in acetone the most common and safest method.
No electrical devices in or next to the box. The SDS asks for explosion-proof electrical equipment and action against static discharge. Prusa warns that a damaged fan inside the box can spark and ignite the fumes. Work away from the printer, and if it is in the same room, switch it off and unplug it.
Ventilate, and remember the vapour sinks. The safety card says a harmful concentration in the air can build up rather quickly at 20 °C. Work outdoors or next to an open window, and keep the box away from anything at floor level that sparks or burns, because the vapour is heavier than air.
Protect your eyes and skin. Acetone causes serious eye irritation and can cause drowsiness or dizziness; repeated contact can dry and crack the skin. Wear safety glasses and gloves that the glove maker rates for acetone.
Keep the quantity small, the bottle closed and out of the room while the part is in the box.
Never leave it unattended, and have a CO2 or powder extinguisher to hand; Fisher's SDS notes that water may be ineffective. If something catches fire and you cannot put it out at once, get out and call 112.
Printing ABS and ASA also releases fumes of its own; see 3D printer fumes and ventilation for what studies measured.
The cold method, step by step
This is the approach Prusa calls the most common and safest, with no heating at all:
Print in ABS or ASA with a fine layer height. Both materials warp, so an enclosure helps; see printing ABS and ASA.
Use a clear glass or polypropylene (PP) box. The safety card notes that acetone attacks plastics, and Prusa warns that an ABS box would dissolve; it uses a transparent PP storage box. A loose lid resting on top is enough. Never use a box with rubber seals or locks.
Raise the part on a platform a few centimetres (Prusa: 1 to 2 inches) above the bottom, so it never touches liquid. Prusa uses an old steel print sheet, which also lets you move the part without touching it.
Line the bottom and sides with paper towels wetted with acetone, without leaving a pool. Close the acetone bottle and take it out of the room.
Close the lid and watch through the side. No maker publishes cold-method times; Prusa's 15 to 40 minutes were measured in a warmed box, so expect longer. Stay with it, check the part regularly, as Prusa advises, and take it out as soon as the surface turns glossy.
Lift the part out on its platform and let it harden in a clean, dry box for at least several hours, preferably a day, so no fingerprints or dust stick to it.
Clean up outdoors. Let the box and towels air out, and treat leftover acetone as chemical waste: the SDS says to dispose of it through an approved waste facility, so follow your council's rules for household hazardous waste. Never pour it down the drain; the SDS says it should not be released into the environment.
Prusa's video accompanies its smoothing article and covers how to smooth ABS and ASA with acetone and how it changes mechanical properties. The article behind it calls warming acetone dangerous; this guide sticks to the unheated method.
When smoothing goes wrong
Acetone smoothing problems and what to do
| What you see | Why | What to do |
|---|---|---|
| Nothing happens after a long time | Not ABS or ASA, or the liquid is not acetone | Check the filament and the label; an accepted Stack Exchange answer warns that some eco cleaners sold like acetone are 2-butoxyethanol, which does not smooth ABS |
| Layers still visible after an hour | Some brands resist; longer exposure only deforms them | Stop; Prusa saw two of ten filaments stay layered |
| Bottom soft, top still layered | Vapour is uneven in a still box, worst on large parts | Smooth smaller parts; for large ones Prusa recommends a professional smoothing station |
| Fingerprints or dust in the surface | The skin is still soft | Handle it only on the platform and let it harden for a day |
| Part twisted or sagged | Thin or flat geometry | Not suitable for vapour; sand and prime instead |
| Fine text or teeth rounded off | Vapour dissolves small features first | Accept it or choose another finish for detailed parts |
If your part is PLA or PETG
Acetone will not smooth PLA: hours of vapour barely softened Prusament PLA in Prusa's tests, and an acetone bath bleached some colours and cracked the parts within hours or days. Prusa says chemical smoothing of PLA works only in a laboratory, with solvents such as chloroform or tetrahydrofuran that only skilled lab technicians should handle. Do not try them at home. These routes give PLA a similar finish:
Sand, prime and paint. Filler primer fills layer lines and gives a paintable surface; grits, primers and clear coats are in sanding, priming and painting PLA.
Epoxy coating. Smooth-On's XTC-3D is a two-part coating you brush on; it levels itself, with a working time of 10 minutes and a cure of about 4 hours according to the maker. It adds material rather than removing it, so it also changes dimensions slightly; read its technical bulletin and SDS first.
A filament made for smoothing. Polymaker's PolySmooth is smoothed with alcohol in its Polysher. Isopropyl alcohol is also highly flammable (flash point 11.7 °C on its ILO/WHO safety card), so the same fire rules apply.
PETG is no easier: Prusa smooths it with dichloromethane, a dangerous solvent, and forum reports of PETG in acetone are inconsistent. Sand and prime PETG instead.
In Smooth-On's own video, XTC-3D epoxy is used to coat a part printed in PLA.
Related guides and next step
If the surface only needs to look even, sanding or a coating keeps the shape under your control; choosing a finish before production walks through that decision. What acetone and other solvents do to each material in use is in chemical resistance of PLA, PETG, ABS and nylon.
If you need an outdoor-grade ASA part rather than a smoothing project, OmniTechs prints ASA on request after a feasibility check.
Sources
Fisher Scientific: Safety Data Sheet, Acetone (revision 18 December 2025)
ILO and WHO: International Chemical Safety Card 0087, Acetone
ILO and WHO: International Chemical Safety Card 0554, Isopropyl alcohol
3D Printing Stack Exchange: Safety precautions when using acetone
3D Printing Stack Exchange: How do I give 3D-printed parts in PLA a shiny smooth finish?
3D Printing Stack Exchange: Maintaining fine details while applying smoothing methods
3D Printing Stack Exchange: Is real PETG softened or degraded by acetone?
3D Printing Stack Exchange: Acetone smoothing not working on ABSPlus-P430
Prusa 3D on YouTube: Improve your prints with acetone smoothing
CNC Kitchen on YouTube: Stronger 3D prints with Vapor Smoothing?