Print ABS without an enclosure? Yes for small parts: limits, settings and fixes
By Sina Esfahani, OmniTechs · Published 27 November 2026
Yes, for small parts. Polymaker's rule: an open printer with the bed at 90 °C and the nozzle at 260 °C handles ABS or ASA models smaller than a fist. Bigger prints need an enclosure at about 40 to 50 °C, and models over about 15 to 20 cm in any direction an actively heated chamber of about 70 °C. Prusa's rule of thumb for ASA is that objects of about 10 × 10 cm print fine.
Bambu Lab supports ABS and ASA only on its enclosed printers. On any printer you need a hot bed, little or no part cooling, no draughts, and fresh air for the room but not across the print.
Set it up in this order:
Size the part: fist-sized, or about 10 × 10 cm, can print open; larger needs an enclosure, and over 15 to 20 cm a heated chamber.
Bed at 90 to 110 °C with glue stick; let it heat for 10 to 15 minutes before printing so the air around it warms up.
Part cooling fan off, or low: Polymaker says off, Bambu Lab's sheets allow up to 80%; keep it off for the first 3 layers, as Bambu Studio does.
Block draughts with a draft shield (PrusaSlicer: Print Settings > Skirt and brim; Cura: Experimental > Enable Draft Shield) and add a brim for corners.
Keep infill at 50% or less and walls at 6 or fewer, and round off sharp corners.
Ventilate the room, not the printer, and never print PLA in the same closed, hot box.
What you see and what to do
ABS and ASA problems, what they mean and what to do
| What you see | What it means | What to do |
|---|---|---|
| Corners lift off the bed | Lower layers shrink while upper ones are still hot | Hotter bed, glue stick, brim; draft shield or enclosure |
| Cracks open between layers, often higher up | Cooling stress is stronger than the bond between layers | Less fan, hotter nozzle or slower print, closed door and lid |
| The print comes loose mid-print | Warping plus a draught or a cold room | Enclosure, brim, longer bed preheat |
| PLA jams after ABS in the same enclosure | Heat creep in a warm box | Open the door or top, or the vent, for PLA and PETG |
| The fan shroud or other printed printer parts soften | The enclosure is too hot for the printer's own plastic | Reprint those parts in a heat-resistant material such as PC |
| A strong smell in the room | Styrene and other fumes from ABS and ASA | More ventilation or filtration; pause if vulnerable people are present |
Enclosure or not: what the makers allow
Enclosure and chamber guidance for ABS and ASA from three makers
| Maker and source | Without an enclosure | With an enclosure or heated chamber |
|---|---|---|
| Polymaker, ABS and ASA product FAQs | models smaller than a fist, with a 90 °C bed and 260 °C nozzle | larger: enclosure at about 40 to 50 °C; over about 15 to 20 cm in any direction: heated chamber of about 70 °C or more |
| Polymaker, ABS and ASA overview | possible, but the larger and denser the part, the more an enclosure matters | air above 45 °C prevents warping and delamination |
| Prusa, ABS guide | the draft shield in PrusaSlicer as a simple alternative | enclosure required; bed at least 100 °C |
| Prusa, ASA guide and blog | objects of about 10 × 10 cm should print fine; draft shield or a skirt as tall as the model | enclosure necessary for large parts; the CORE One chamber reaches up to 55 °C |
| Bambu Lab, wiki and datasheets | not supported: not compatible with the open P1P or A series | chamber 45 to 60 °C; close the front door and top cover |
Forum experience sits closer to Polymaker. The accepted answer to "Is there a way to print with ABS without enclosure?" on Stack Exchange: the heated bed matters more than an enclosure, and a warm, draught-free room is fine for parts a few centimetres high, with the part cooling fan off.
A Prusa XL owner tested exactly this with ASA, using a cheap shower-curtain liner as a draught screen; the start time is the chapter that asks whether enclosures are necessary.
Why ABS and ASA lift and crack
ABS and ASA shrink as they cool from about 260 °C to room temperature; Prusa puts the shrinkage of ABS at about 1 to 2%. When the lower layers cool and shrink while the upper ones are still hot, the stress pulls corners off the bed or tears layers apart. Bambu Lab adds that, because of their high glass transition temperature, cool surroundings build up significant internal stress. The root cause is uneven temperature across the part.
That is why size and infill matter. More material means more shrinking force, so Bambu Lab advises against infill above 50% and more than six walls. Prusa notes that round bases spread the force better than square ones. General warping causes, from brims to part design, are in stop 3D prints warping.
Settings to start from
Where to start: ABS and ASA settings from makers and slicer profiles
| Source | Nozzle (°C) | Bed (°C) | Part cooling fan | Chamber |
|---|---|---|---|---|
| Prusa guides, ABS and ASA | 255 (ABS), 260 (ASA) | ABS 100, 80 to 110 by size; ASA 105 first layer, 110 after | not stated | enclosure for ABS; for large ASA parts |
| Polymaker PolyLite ABS and Polymaker ASA | 245 to 265 (ABS), 230 to 260 (ASA) | 90 to 100 (ABS), 75 to 95 (ASA) | off | enclosure needed |
| Bambu Lab ABS and ASA datasheets V3.0 | 240 to 270 | 80 to 100 | 0 to 80% | 45 to 60 °C |
| Bambu Studio profile, Bambu ABS on the X1C | 260 first layer, 270 after | 90 | 10 to 60%, 80% on overhangs, off for the first 3 layers | air filtration on |
| Bambu Studio profile, Bambu ASA on the X1C | 270 | 100 | 25 to 35%, 80% on overhangs, off for the first 3 layers | air filtration on |
ASA nozzle and bed values from four makers are in the datasheet comparison.
Where to change the fan: in Bambu Studio and OrcaSlicer, edit the filament preset, Cooling tab (minimum and maximum fan speed thresholds, no cooling for the first layers). In PrusaSlicer it is Filament Settings > Cooling; Prusa notes that "keep fan always on" is normally off for ABS, ASA and PC.
Practical points from the same pages:
Warm the chamber with the bed. Polymaker heats the bed to 90 to 100 °C for 10 minutes before printing; Bambu Lab preheats the bed of its X1C and P1S at maximum for 15 minutes when the room is cold.
Hotter and slower bonds better. Polymaker notes that layer adhesion improves when you print hotter and slower, at the cost of uglier overhangs.
Help the first layer. Prusa and Bambu Lab use glue stick on the plate, Bambu Lab adds a brim. Prusa warns never to put acetone or ABS slurry on its powder-coated sheets. Brim and draft-shield options are compared in raft, brim or skirt.
Check the hotend. Polymaker recommends an all-metal hotend above 240 °C; see all-metal or PTFE-lined hotend.
Dry the spool. Bambu Lab gives about 80 °C for 8 hours for ABS, ASA and PC; Polymaker 70 °C for 6 hours for PolyLite ABS.
Worked example: an 18 cm ASA part on an open printer
You need an ASA cover of 18 × 12 × 6 cm and you have an open bed-slinger.
Check the size. 18 cm is past Prusa's 10 × 10 cm and far past Polymaker's fist rule. It sits in Polymaker's 15 to 20 cm band, where Polymaker starts asking for an actively heated chamber of about 70 °C.
Option A: split it. Two halves of 9 × 12 cm come close to Prusa's open-printer size. Plan the joint first; see split a large 3D model for assembly.
Option B: enclose it. In an enclosure, preheat the bed at 90 to 100 °C for 10 minutes, keep the fan off for the first layers, infill at 50% or less, and a brim on the corners.
Either way: draft shield on, no air across the print, and round off the corners in CAD if you can.
Cracks between layers
Cracks that open between layers are the other typical ABS and ASA failure. Bambu Lab's diagnosis: the stress from cooling exceeds the adhesion between layers. Its fixes, in order:
Make sure the filament melts fully: raise the nozzle temperature or slow down, and clear a partial clog.
Cool less: turn the part cooling fan down.
Keep the chamber warm: raise the bed temperature and close the front door and top cover.
Make the part stronger: add walls or infill, within the limits above.
Thomas Sanladerer tested whether a hotter nozzle or a hotter environment helps ABS more; his description opens with the conclusion that you should probably use a heated or enclosed chamber.
The wider causes of weak layer bonding are covered in layer separation and poor layer adhesion.
What an enclosure does to PLA, the printer and the room
PLA and PETG jam in a hot box. Prusa lists an enclosure, or a room above 35 °C, as a common cause of heat creep, and says PLA in a fully closed, unventilated enclosure is very likely to cause problems. Bambu Lab opens the door and top cover only for PLA, PETG and TPU. Prusa's CORE One has a vent you open for PLA and close for ABS and ASA. See heat creep jams explained.
Printer parts soften. Prusa warns that printing ABS or ASA in an enclosure can deform the fan shroud and other printed parts, and suggests reprinting them in a more heat-resistant material such as its PC Blend.
Electronics overheat. Bambu Lab requires a control-board fan when you enclose its open P1P, because the board's heatsink was designed for open air.
Fumes still need somewhere to go. Prusa says ABS and ASA release fumes, including styrene, that could pose a health risk. Bambu Lab adds: wear a mask with vapour filtration such as activated carbon for long jobs, avoid long prints in bedrooms or living rooms, and ventilate more or pause when people with asthma, pregnant women or children are present. See 3D printer fumes, ultrafine particles and ventilation.
When to stop
Cracks persist with the fan off, a hot bed and a closed chamber. The part is too large or dense for your chamber. Split it, thin the infill, or use a heated chamber.
You are about to box in an open printer. Follow the maker's enclosure instructions first; Bambu Lab's P1P needs its control-board fan. Switch the printer off and unplug it before you fit a fan, a panel or a reprinted part. Forum answers on building enclosures recommend non-combustible materials, because a printer fault can start a fire.
You want to leave it running. An enclosure does not make unattended printing safe; see leaving a printer running unattended.
Someone in the room feels unwell. Stop the print and ventilate.
Next step and related guides
For acetone smoothing of ABS and ASA, see vapour smoothing ABS and ASA.
If ASA is what your part needs but an enclosure is not something you want to build, OmniTechs prints ASA on request on an enclosed printer after a feasibility check.
Sources
Prusa Knowledge Base: Extrusion stopped mid-print (heat creep)
3D Printing Stack Exchange: Is there a way to print with ABS without enclosure?
3D Printing Stack Exchange: Enclosure, things to pay attention to?
Robert Cowan video: Printing ASA on the Prusa XL -Are Enclosures Necessary?
Made with Layers video: 3D printing with ABS: Hotter nozzle or hotter ambient? #Filaween