Pillowing on 3D prints: close the holes in your top surface, then make it smooth

By Sina Esfahani, OmniTechs · Published 27 November 2026

Pillowing is the bumpy, sometimes holey top surface you get when the first solid layers over sparse infill sag into the gaps and the layers above cannot close them. The first solid layer is essentially a bridge over the infill pattern, so some sag is normal; the lower the infill density, the longer each span and the bigger the sag (Prusa).

The fix is structural. Give the top enough solid thickness, give those layers something to rest on, and cool them. If gaps remain between otherwise neat lines, check flow. Monotonic lines and ironing come last: they improve a top that is already closed, but ironing does not fill holes left by too few top layers.

Fix it in this order:

  1. Give the top about 0.8 mm of solid layers or more: 4 layers at 0.2 mm, 8 at 0.1 mm.

  2. Still holes: raise the infill from 15% to 20 to 30%, or only under the top with a modifier.

  3. In Cura, keep Infill Skin Support on; in OrcaSlicer, switch on Extra bridge layers.

  4. Cool the top: part fan high, a minimum layer time (Cura uses 5 seconds), and no hotter than the filament needs.

  5. Gaps between neat lines: calibrate flow and check the slicer's nozzle size.

  6. Ridges where lines meet: set the top pattern to monotonic.

  7. A flat top that must shine: iron it; Cura starts at 10% flow and 0.1 mm spacing.

What is wrong with your top surface?

Top surface faults and their usual causes

Causes and fixes as described by Prusa, Simplify3D, Bambu Lab, OrcaSlicer and in answers on the 3D Printing Stack Exchange, read 27 November 2026.
What you seeUsual causeFirst fix
Bumps or small holes that follow the infill pattern (pillowing)Too thin a top, too sparse infill, too little coolingMore top thickness, denser infill under the top
Gaps between neat, separate linesUnder-extrusion, flow too low, wrong nozzle size in the slicerFlow calibration, slicer nozzle setting
Ridges or shiny stripes where line directions meetLines printed back and forthMonotonic top pattern
Marks from the layer below showing throughInternal solid infill paths meeting under the topMonotonic layer under the top; if marks stay, check for backlash
Scratches or lines across a finished topTravel moves dragging over itSee the nozzle collision guide
Wavy wrinkles across a large flat topHotend temperature and fan settingsLower nozzle temperature, adjust the fan
Small tops come out soft, rounded and mushyLayer prints too fast to coolMinimum layer time
Holes on gently sloped tops such as domes or headsThin shell on slopes, small internal bridges filtered outEnsure vertical shell thickness, internal bridge settings

Scratches from travel moves have their own guide: nozzle hitting or dragging across the print.

How many top layers do you need?

Think in thickness, not in layer count: the same count gives a much thinner top at a fine layer height.

Published guidance on top thickness

Values from the Prusa Knowledge Base, Simplify3D print quality guide, OrcaSlicer wiki and Cura setting definitions, read 27 November 2026. Printer profiles may use other defaults.
SourceGuidance
PrusaAt least 3 top layers; at 0.3 mm layer height use 3, at 0.1 mm use 9 for the same thickness
Simplify3DSolid top at least 0.5 mm thick: at least 2 layers at 0.25 mm, about 5 at 0.1 mm; if 3 layers show gaps, try 5
OrcaSlicerAt least 3 shell layers for most prints; Top shell thickness adds layers when the count alone is too thin
Cura base settingsTop Thickness 0.8 mm; the layer count is that thickness divided by the layer height, rounded up

Where to set it: PrusaSlicer, Print Settings > Layers and perimeters > Solid layers (Top) and Minimum shell thickness; Bambu Studio, Strength > Top shell layers; OrcaSlicer, Strength > Top/bottom shells > Top shell layers and Top shell thickness; Cura, Top/Bottom > Top Thickness.

Worked example: switching to 0.12 mm layers

Say your profile prints 4 top layers. At 0.2 mm that is 0.8 mm of solid top. Switch to 0.12 mm layers and the same 4 layers give only 0.48 mm, below Simplify3D's 0.5 mm minimum, and pillowing appears. Set a thickness of 0.8 mm instead: 0.8 ÷ 0.12 = 6.7, rounded up to 7 layers, or 0.84 mm. That is exactly how Cura counts, and what OrcaSlicer's Top shell thickness and PrusaSlicer's Minimum shell thickness do for you. The layer height guide explains the trade-off of finer layers.

One solid layer over infill is never enough: the accepted answer to a Stack Exchange question about a box whose first top layer fell apart says it takes at least two, and three look really good.

Give those layers something to rest on

If more top layers do not help, the infill underneath is too sparse. Simplify3D's example is going from 30% to 50%; on the Stack Exchange, an answer about a messy PETG top called 15% very low and suggested 20 to 30%.

You do not have to fill the whole part. Prusa suggests a modifier that raises the infill only for the last few layers before the top; slicer modifiers shows how to set one up, and infill patterns compared covers which patterns support a top best.

The slicers can also add structure directly under the top:

  • Cura: Infill Skin Support (Infill section) prints a solid pattern just below the skin so it is not printed over air. In Cura's base settings it switches on by itself below 40% infill (without gradual infill), and since Cura 5.12 it replaces the older skin-support options.

  • OrcaSlicer: Extra bridge layers (Quality > Bridging) prints a second bridge layer, which the wiki says reduces pillowing; the internal option targets bridges over sparse infill. The wiki recommends at least External bridge only, and keeping Thick internal bridges on. Filter out small internal bridges, set to Limited filtering, helps on heavily slanted or curved models.

  • Bambu Studio: the single layer directly under the top is printed monotonic by default, so marks from the internal solid infill do not show through. If marks persist after that, Bambu Lab says the cause is more likely machine backlash than flow.

  • PrusaSlicer and Bambu Studio: Ensure vertical shell thickness adds solid infill near sloping surfaces. Prusa says it fixes the classic holes on top of printed heads and busts.

MatterHackers' short troubleshooting video explains pillowing and how to avoid it.

3D Printing Troubleshooting Guide: Pillowing (MatterHackers)

Cool the top layers, and watch the temperature

The first top layers are bridges, and bridges need cooling. Two Stack Exchange cases show both sides of it. A Prusa MK3 owner printed PLA at 235 °C and got wrinkled tops; the accepted answer names hotend temperature and fan settings together, and the owner reports that lowering to 205 °C with the fan at 100% made it acceptable. For small tops that come out soft and mushy, the accepted answer is a minimum layer time, so each layer can set before the next. Cura's base settings use 5 seconds, and Bambu Studio's Slow printing down for better layer cooling slows each layer to its target time, down to a minimum print speed.

Monotonic lines and a single wall on top

When neighbouring top lines run in opposite directions, ridges appear where they meet. A monotonic pattern always lays lines in one direction, which gives an even sheen (Prusa); Original Prusa profiles use it for top layers by default. OrcaSlicer calls Monotonic line usually the best choice for top surfaces. In Cura, Monotonic Top Surface Order is on in the base settings, but it only applies once Top Surface Skin Layers is set to 1 or more.

Bambu Studio's Only one wall on top surfaces, on by default, and PrusaSlicer's Single perimeter on top surfaces give flat tops a cleaner outline.

Ironing: when it helps and what it costs

Ironing runs the hot nozzle over the finished top layer again at the same height while extruding very little. The heat flattens the lines and the small flow fills the grooves. Prusa runs the ironing pass at a fixed 45° to the top lines.

Use it for flat tops such as nameplates, badges, lids, box tops and faces you will glue. Skip it for round, organic or angled tops: Prusa says it has little to no effect there, and Bambu Lab says it cannot smooth the steps on a curved top. Printing the part upside down often gives an even smoother face from the build plate (Prusa).

Where to switch it on: PrusaSlicer, Print Settings > Infill > Ironing (Advanced or Expert mode), with the speed under Print Settings > Speed; Bambu Studio and OrcaSlicer, Quality > Ironing type; Cura, Top/Bottom > Enable Ironing.

Know the costs first:

  • Time. The passes are slow and closely spaced; a large top adds a lot of print time.

  • Heat creep. The tiny, slow extrusion can soften filament above the melt zone and clog the hotend. Prusa names PLA as most prone, Bambu Lab adds PETG and TPU, and OrcaSlicer advises watching the printer while it irons.

  • Edges and adhesion. Edges get slightly fuzzy (Prusa). The nozzle presses harder on the part, which can knock off a print that is poorly attached (Bambu Lab).

  • Calibration. Ironing is very sensitive to flow: too little leaves shiny grooves, too much drags plastic to the edges (Prusa). PETG is more likely to stick to the nozzle; ASA irons very well.

Ironing settings in four slicers

From the Prusa Knowledge Base, Bambu Lab Wiki, OrcaSlicer wiki and Cura setting definitions, read 27 November 2026. Only Cura's base file publishes default numbers; the others leave them to the printer profile.
SettingPrusaSlicerBambu StudioOrcaSlicerCura base settings
What gets ironedAll top surfaces, topmost only, or all solid layersTop surfaces, topmost, or all solid layersAll top, topmost only, or all solid layersTop surfaces, optionally only the highest layer
PatternLines at 45° to the top infillRectilinear, concentric or Archimedean spiralRectilinear or concentricZig zag or concentric
Line spacingSmaller than the nozzle diameterSmaller than the nozzle diameterEqual to or less than the nozzle diameter0.1 mm
FlowPercentage of a normal layerRelative to a normal layerPercentage of a normal layer10% of a normal skin line
Edge insetNot listedIroning inset, since 1.100 means half the nozzle diameterCalculated from line widths

If ironing leaves lines between separately ironed areas, an answer on the Stack Exchange points to travel moves: in Cura, set Combing Mode to Not in Skin or try the concentric ironing pattern. Cura already switches combing to Not on Outer Surface when ironing or monotonic tops are enabled.

Prusa's ironing guide shows when to use it, the settings, modifiers and the downsides, with a calibration chapter from 9:50.

Guide to Ironing. How to make top surfaces smooth with PrusaSlicer (Prusa 3D)

When to stop tuning

If the top is thick enough, well supported and cooled, and still shows gaps between neat lines, the extruder is not delivering what the slicer asks for. Bambu Lab names a partly clogged nozzle, debris in the extruder and extra drag in the filament path, and asks you to clear those before you calibrate flow; see flow rate calibration. If ironing keeps clogging the hotend, stop ironing large areas and read up on heat creep.

If the face that matters could be printed against the plate instead, choosing 3D-print orientation helps you weigh that against strength and supports. For tops that sag over a real opening rather than over infill, overhangs and bridges without sagging covers bridge settings.

If you need a part with a clean finish rather than the tuning, the 3D printing service prints PLA and PETG parts from your file.