Best glue for PLA, PETG, ABS and TPU: what actually holds each filament

By Sina Esfahani, OmniTechs · Published 27 November 2026

For PLA and PETG, use a cyanoacrylate glue (superglue, CA) on clean, close-fitting faces. In Prusa's quick tensile test of twelve glues, CA gave the strongest joints on PLA, PET and ASA, about 10 to 13 MPa. Use a two-part epoxy when the faces do not meet well and the glue has to fill a gap.

ABS and ASA can also be welded with acetone for a seam that disappears; PETG and TPU cannot. For TPU, use a CA made for flexible bond lines. Whatever you choose, preparation decides more than the brand: sand, clean, clamp, wait for the full cure, and test a sample joint first.

Glue it in this order:

  1. Choose by filament: CA for PLA, PETG, ABS and ASA; epoxy where the faces do not meet; a flexible CA for TPU.

  2. Sand both faces lightly, then remove the dust and any grease (Prusa).

  3. Dry-fit the parts: CA cures fastest in a thin bond line (Henkel).

  4. Glue at about 22 °C and 40 to 60 % relative humidity; in dry air, a light water mist or an activator speeds up the cure (Henkel, Prusa).

  5. Press the parts together at once; if the fit is wrong after a few seconds, clean the glue off and start again (Prusa).

  6. Wait 24 to 72 hours before loading the joint (Henkel, for Loctite 406).

  7. Ventilate and wear eye protection; keep acetone away from flames (safety data sheets).

Which glue for which filament

Adhesives by filament

Summarised from Prusa's gluing guide and material pages and Henkel's Loctite data sheets, read on 27 November 2026.
FilamentFirst choiceAlso worksWatch out for
PLACA: thin for tight joints, gel when you need a few seconds to positionTwo-part epoxy for gaps; welding with PLA filamentAcetone glues only some PLA; test an offcut
PETGCATwo-part epoxyNo solvent a hobbyist can buy attacks it (Prusa)
ABS and ASACA for strength; acetone or a plastic cement for a seam that disappearsTwo-part epoxyAcetone is highly flammable; one model cement Prusa tried did not glue ASA at all
TPUA flexible CA such as Henkel's Loctite 4850, or a rubber-filled CAPlain CA where the faces are fairly stiff; contact adhesive, which Prusa did not testTPU resists various solvents (Prusa); try an offcut first

Prusa's test shows how far apart the glue types are:

Best result per glue type in Prusa's tensile test

Prusa's test of twelve glues on printed samples, one sample per glue, in its 2021 gluing guide, read 27 November 2026. Prusa calls it a very quick overview, not a controlled test. Pure acetone was not tested.
MaterialBest CABest two-part epoxyBest solvent cement
PLA10.2 MPa6.3 MPa4.9 MPa
PETG (listed as PET)13.1 MPa5.1 MPa4.8 MPa
ASA11.3 MPa2.7 MPa7.4 MPa

Two things stand out. CA won on all three plastics, including ASA, where solvent cements are the classic choice. And the brand mattered: on PET the CA glues ranged from about 4.5 to 13 MPa. Prusa's best results came from a cheap Alteco tube and a local modelling-shop CA, not from specialist products.

Prepare the faces first

Make the mating faces as clean and level as possible, sand them lightly, then remove the sanding dust, grease, paint and old glue. Those are Prusa's rules for every adhesive, and Henkel's data sheet for Loctite 406, a CA for plastics and rubbers, starts with the same clean, grease-free surfaces. Alignment pegs make the joint stronger and easier to place (Prusa).

Fit matters as much as cleanliness. Henkel notes that CA cures fastest in thin bond lines and more slowly as the gap grows, and Prusa warns that thick superglue does not suit rough surfaces. PLA, PETG and ABS need no primer: Henkel's Loctite SF 770 primer is meant for low-energy plastics such as polyethylene, polypropylene, PTFE and thermoplastic rubber, and those three are not on its list.

Superglue (CA): give it moisture and time

CA cures with moisture from the air. Henkel gives 40 to 60 % relative humidity at 22 °C as the best range for Loctite 406; drier air slows the cure. Prusa speeds it up with an activator or plain water from a spray bottle. Both work, but Henkel says an activator and high humidity can each lower the final strength, and Prusa warns that an activator's heat can deform PLA.

  • Thin or gel. Gel CA sets a little more slowly, so it is easier to position, but it is slightly weaker and frosts more (Prusa). Extra-thin CA wicks into a joint that is already pressed together.

  • Full strength takes time. Prusa sees maximum hardness after 8 to 24 hours; Henkel gives 24 to 72 hours before loading.

  • Heat and cold. Regular CA reportedly keeps about 50 % of its strength at 80 °C and 20 % at 100 °C, and turns brittle when frozen (Prusa).

  • Peel and twist. CA has high tensile strength but low shear and torsion strength, so a CA joint is much easier to twist or peel than to pull apart (Prusa).

In this sponsored video, Thomas Sanladerer of Made with Layers asks whether PLA and PETG prints are really hard to glue, and tries products including JB Weld, superglue and VHB tape.

Which glues work on 3D prints? JB Weld / Superglue / VHB tape… (Made with Layers (Thomas Sanladerer))

Two-part epoxy for gaps and rough faces

Henkel describes its Loctite EA 3430 epoxy as suited to rough and poorly fitting surfaces of rigid plastics, because it fills gaps. Its data sheet also shows the practical limits of a fast epoxy: mixed one to one, 4 minutes of working time at 22 °C, fixture strength after 15 minutes, and no batches over 20 g, because a larger mass heats up. Prusa adds that epoxies cure in anything from under 90 seconds to over 12 hours, and that slower ones usually give a stronger, less brittle bond.

Prusa also combines the two: tack the parts in place with a few dots of CA, then fill the rest of the joint with epoxy. On strength, keep the test table in mind. The 5-minute epoxies Prusa tried reached about half the strength of the best CA on PLA, about a third on PETG and about a fifth on ASA.

Solvent welding: ABS and ASA yes, PETG no, PLA maybe

A solvent glue softens both faces so they fuse when it evaporates. Prusa lists acetone for ABS and ASA, limonene for HIPS and isopropyl alcohol for PVB. PETG, it says, is inert to all chemicals normally available to a hobbyist; dissolving it is a laboratory job with dichloromethane. Prusa's page on flexible filaments notes that TPU resists various solvents as well.

PLA is where Prusa's own pages disagree. Its gluing guide says PLA can be glued with acetone just fine. Its PLA material page says only some PLA filaments can be partly dissolved and glued with acetone. Thomas Sanladerer put this question to the test on video. Treat acetone on PLA as something to try on an offcut of your own filament.

Does Acetone also work for welding and smoothing PLA 3D printed parts? (Made with Layers (Thomas Sanladerer))

For a clean seam, Prusa uses capillary gluing: press the parts together and brush a thin solvent along the joint, so the gap draws it in. Clamp the parts and expect the joint to sink a little as the solvent evaporates. A large joint can take days to cure fully. Smoothing ABS and ASA with acetone vapour is a separate process, covered in vapour smoothing ABS and ASA.

Welding with the filament itself

You can also join prints with their own plastic. The accepted answer to "What glues for bonding printed PLA to injection-molded plastic?" on the 3D Printing Stack Exchange melts PLA filament into cavities on both parts with a temperature-controlled soldering iron at around 200 °C. It also describes friction welding with filament spun in a rotary tool. Work with extraction, and for ABS with respiratory protection, the answer warns. Do not tack the parts with CA first: the same answer notes that heated CA breaks down into a noxious fume. What heated plastics release is covered in 3D printer fumes and ventilation.

The 3D Printing Nerd shows friction welding: filament in a rotary tool spins fast enough to melt itself into the seam.

3D Printing and Friction Welding: Attaching 3D Printed Parts with Heat (3D Printing Nerd)

Frosting, spills and undoing a joint

The white bloom around a CA joint comes from the glue's fumes settling on the part. Prusa says it is worst when the fumes cannot escape, for example in a closed box, and that strong ventilation reduces it. Odourless CA does not frost at all, which suits clear parts such as visors and windows (Prusa). Once frosting is there, answers to "How can cyanoacrylate haze be removed from PLA?" on the 3D Printing Stack Exchange report that a wipe with petroleum jelly or a light oil hides it, while solvents can make it worse on some PLA.

To undo a CA joint, use a CA debonder or acetone, which dissolve cured CA. Prusa advises testing the reaction on your plastic first, because some debonders also attack the print. Cured epoxy does not dissolve like this; Prusa could at best soften it and scrape it off.

Safety data sheet precautions

Read the safety data sheet of the product you buy; the classifications below show what to expect.

Hazard statements for common gluing chemicals

EU harmonised classifications as listed by PubChem, and Smooth-On's XTC-3D safety data sheet (revision 24 February 2023), read on 27 November 2026. Check your own product's sheet.
SubstanceHazard statementsPrecautions
Ethyl cyanoacrylate (CA)H315 skin irritation, H319 serious eye irritation, H335 respiratory irritationVentilate, protect eyes and fingers; it bonds skin
AcetoneH225 highly flammable, H319 serious eye irritation, H336 drowsiness or dizzinessNo flames or sparks nearby, ventilate, eye protection
Epoxy hardener (example: Smooth-On XTC-3D Part B)H314 severe burns and eye damage, H302 and H332 harmful, H361 suspected of damaging fertility or the unborn child, H410Gloves, eye protection, ventilation; the resin part may also sensitise skin (H317)
DichloromethaneH351 suspected of causing cancerPrusa treats it as a laboratory solvent; not for gluing at home

Prusa adds that CA fumes can irritate eyes and nose in a poorly ventilated room, and that CA can react hot with cotton or wool.

Design the joint, then test it

Because a CA joint twists and peels far more easily than it pulls apart, give the glue faces that are loaded in tension and add pegs that take the shear. Decide the seam when you split the model; splitting a large 3D model for assembly covers where to put it.

Worked example: adding pegs to a butt joint

A bracket split across a 20 × 10 mm face has 200 mm² of glue area. Two pegs of 5 mm diameter, 6 mm deep, add 2 × π × 5 × 6 ≈ 188 mm² of side wall. That almost doubles the glued area, and the pegs locate the parts and carry the shear that CA handles worst. Give the peg holes a little clearance, or the parts will not close and the glue line gets thick.

Then glue two offcuts with the same filament, surface and glue, wait the full cure time, and load them the way the real part will be loaded. What to record, and when to stop, is in testing a glued PLA joint. If you would rather receive the printed parts and glue them yourself, the 3D printing service prints PLA and PETG parts from your file.