First layer not sticking to the bed? Fix it in this order
By Sina Esfahani, OmniTechs · Published 27 November 2026
A first layer that will not stick nearly always has one of three causes: grease on the plate, a nozzle that sits too high, or a slicer profile made for a different plate or filament. Bambu Lab finds that washing the plate solves most adhesion problems once the plate type and settings are right.
So wash the plate first. Then check the profile, then judge the nozzle height on a one-layer test. Only after that slow the first layer down, switch the fan off and add a brim or glue. Change one thing per test print, so you know what worked.
Do not force grip by pressing the nozzle harder into the plate. Prusa warns that an over-squashed first layer can damage the sheet, and its warranty does not cover that damage.
Fix it in this order:
Clean the plate the way its maker says (Bambu Lab: warm water and washing-up liquid; Prusa: 90% isopropyl alcohol), then hold it only by the edges.
Select the plate that is really on the printer in the slicer; Bambu Lab's Textured PEI profile also lowers the nozzle by 0.04 mm.
Print a one-layer test and lower the nozzle in 0.02 to 0.05 mm steps until the lines touch without gaps.
If one area still fails after cleaning, run bed levelling again.
Print the first layer at 30 mm/s or less and keep the part fan off for the first 3 layers.
For a material that still lets go, raise the bed temperature by 5 °C, at most 10 °C.
Add a brim of at least 3 mm for small footprints, and glue only where the plate maker advises it.
What your first layer is telling you
Look closely at the first layer, or at the skirt that prints before it. The pattern usually points to one cause.
First-layer symptoms and what to do
| What you see | What it means | What to do |
|---|---|---|
| Round lines with gaps between them, across the whole plate | The nozzle is too high | Lower the Z offset in 0.02 to 0.05 mm steps |
| Lines squashed thin, ridges, nozzle scraping, little plastic coming out | The nozzle is too low | Raise it; then look for the real cause of poor grip |
| Good almost everywhere, loose patches or fingerprint shapes | Grease on the plate | Wash the plate; hold it by the edges |
| Good on one side, thin or loose on the other | The bed is not level, or something lies under the sheet | Clean under the sheet, then level again |
| Worked until you changed plate or filament | The slicer profile does not match | Select the right plate and filament profile |
| Lines dragged round corners or torn off at the start | Too fast, or the fan cools the first layer | Slow to 30 mm/s; fan off for 3 layers |
| First layer fine, but corners curl or the part pops off later | Shrinkage or too little contact area | Brim, then the warping guide |
| Thin, broken or patchy lines, also in the skirt | Too little plastic: partial clog or damp filament | See the under-extrusion guide |
Ricky Impey's video goes through seven factors that affect first-layer adhesion. It is a good overview before you start changing settings one by one.
Wash the plate first, even if it looks clean
Skin oil is invisible on the plate and very visible in the first layer. Bambu Lab calls fingerprints and grease the number one cause of prints that slide or pop off. One touch is enough.
How you clean depends on the plate. Bambu Lab washes its plates with warm water and washing-up liquid; on a textured plate, alcohol can spread the oil around the texture instead of removing it. Prusa wipes its sheets with 90% isopropyl alcohol and warns against alcohol sold for skin, which can contain oils. Acetone is allowed on Prusa's smooth PEI only, and never on textured or satin sheets. The full routine per plate is in the guide to cleaning PEI, textured and glass plates.
After washing, hold the plate by its edges. Prusa adds that you do not need to clean before every print as long as nobody touches the surface.
Check that the slicer knows which plate is on the printer
The slicer picks the bed temperature, and on some printers the nozzle height, from the plate you select. A mismatch looks exactly like bad adhesion.
Worked example. You print PLA on a Bambu Lab Textured PEI Plate, but the slicer is still set to the Cool Plate. Bambu Lab's numbers: the Cool Plate profile heats the bed to 35 °C for PLA, while the textured plate needs 55 to 65 °C. On top of that, the printer lowers the nozzle by 0.04 mm only when the textured plate is selected, so the first layer also prints too high. Selecting Textured PEI Plate fixes both at once.
Prusa printers that use steel sheet profiles store a separate first-layer value per sheet, up to eight. The printer cannot sense which sheet is fitted, so the selected profile has to match the sheet.
Also check that the sheet lies flat. Prusa lists a leftover strand of filament or a crumb under the sheet as a cause of an uneven first layer.
Is the nozzle too high or too low?
Print one layer that covers most of the plate. Bambu Lab uses a 0.2 mm thick cube scaled to the bed; Prusa's printers print their own calibration pattern.
Too high: the plastic lands as round strands that barely touch the plate or each other. You see gaps between the lines.
Too low: the lines are squashed flat, ridges form between them, edges curl up, and in the worst case almost no plastic comes out, which can block the nozzle.
Right: flat lines that just touch, with no gaps and no ridges.
Change the height in 0.02 to 0.05 mm steps (Marlin) and print the test again. Prusa adds an important check: if the pattern looks right and prints still do not stick, the problem is elsewhere, such as a greasy sheet, the print settings, levelling or under-extrusion. How to set and save the value on Marlin, Klipper, Prusa and Bambu Lab printers is in the guide on how to set the Z offset.
Only one area fails
A first layer that is perfect in the middle and loose in one corner is not a nozzle-height problem. Clean that area first: Bambu Lab finds that poor adhesion in specific places is mostly a dirty or oily plate. If cleaning changes nothing, run bed levelling again. On older Prusa printers, Bed Level Correction lifts or lowers each side by up to 0.1 mm. The difference between turning the bed screws and letting a probe measure a mesh is explained in bed levelling: manual tramming versus an automatic mesh.
Slow down and keep the fan off before you add heat
A slow first layer gives the plastic time to bond. Bambu Lab recommends an initial layer speed of 30 mm/s or less and an initial layer infill speed of 60 mm/s or less. Prusa suggests turning the printer's knob to about 75% speed for the first three layers.
The part-cooling fan works against adhesion at the start. Bambu Lab's fix for a first layer that will not stick is no cooling for the first 3 layers; Prusa says 1 to 5 layers without the fan helps many filaments.
Where the first-layer speed and fan settings live
| Slicer | First-layer speed | Fan off at the start |
|---|---|---|
| Bambu Studio | Process, Speed tab: Initial layer and Initial layer infill | Filament settings, Cooling tab: No cooling for the first X layers |
| OrcaSlicer | Process, Speed: Initial layer speed | Filament settings, Cooling: No cooling for the first |
| PrusaSlicer | Prusa's advice: turn the printer knob to about 75% for the first three layers | Filament Settings, Cooling: Disable fan for the first X layers (Expert mode) |
| UltiMaker Cura | Speed: Initial Layer Speed | Cooling: Initial Fan Speed, 0% by default |
Temperature comes after that. Start from the filament profile's own values. For a new material that does not stick, Prusa suggests raising the bed by 5 to 10 °C, and Bambu Lab gives the same step for PLA corners that lift. Do not keep going: Bambu Lab warns that a bed that is too hot gives PLA and PETG elephant's foot and can cause clogs. Published bed temperatures per material and plate are in the article on heated bed temperatures for PLA and PETG.
If problems remain on a Bambu Lab printer, Bambu Lab suggests a wider, thicker first layer: 0.5 mm line width and 0.25 mm layer height. Line width is under Process, Quality, Line width, Initial layer. Limits for other nozzles are in the nozzle size, layer height and line width reference.
Brim or glue: which one, and on which plate?
Try a brim before any adhesive (Prusa). The force that holds a print down is roughly proportional to its contact area (Bambu Lab), and a brim adds area exactly where small or tall parts need it. Prusa advises at least 3 mm; for PLA corners that lift, Bambu Lab uses 8 to 10 mm. Settings and clean removal are in raft, brim or skirt.
Glue does two different jobs. It adds grip, and on some plates it is a separating layer that stops a material bonding so hard that the surface tears.
When the makers advise glue
| Plate | PLA | PETG, ABS, ASA and similar |
|---|---|---|
| Prusa smooth PEI sheet | Not needed | Advised as a separating layer; PETG can bond hard enough to damage the sheet |
| Bambu Lab Smooth PEI Plate | Not needed | Must be applied for every filament except PLA |
| Bambu Lab Textured PEI Plate | Generally not needed | Optional, to make PETG easier to remove |
| Bambu Lab Engineering Plate | Advised before every print | Advised before every print |
| Bambu Lab Cool Plate SuperTack | Not needed | Not needed |
A plain PVA glue stick is enough (Prusa). Apply a thin, even layer: Bambu Lab notes that thick blobs give an uneven first layer. Never put superglue on a sheet.
It always stuck, and now it suddenly doesn't
Something changed, even if you did not notice it. Work through these in order.
The profile. If an old G-code file still prints well, compare its bed temperature, nozzle temperature and first-layer settings with the new file. An answer on the 3D Printing Stack Exchange suggests exactly this, and it quickly shows a changed profile.
The plate. Fingerprints build up with every print you remove. Removing prints can also slowly disturb the levelling (same answer).
The nozzle and hotend. Bambu Lab's checks: a nozzle that is not clamped firmly, or loose heater screws on an A1, spoil the height measurement. Prusa lists a full or partial clog. Before you check the nozzle or the screws, let the printer cool to room temperature, switch it off and unplug it; Prusa asks for a cold printer that is off before any nozzle check.
The filament. Damp filament extrudes unevenly (Bambu Lab).
The room. Below 20 °C, even PLA and PETG can lift, and a draught from a window or a fan cools one side of the plate (Bambu Lab). Close the window or the enclosure.
Thin, patchy lines point to too little plastic rather than adhesion; the under-extrusion guide covers that path.
When to stop adjusting
Look at how the print fails before you change more settings. Corners that curl up as the part grows are warping, caused by the plastic shrinking as it cools; see how to stop 3D prints warping. A tall, thin part knocked over by the nozzle is a speed and support question, which Bambu Lab treats separately from adhesion.
Stop and look at the plate itself when a clean plate, the right profile, a correct nozzle height and a fresh levelling run still give poor grip. Coatings wear out. Prusa treats its sheets as consumables whose coatings diminish over time, and says a smooth PEI sheet can be revived after one to two years with light sanding at 600 to 1000 grit. Prusa's sheets are double-sided, so try the other side before you buy a new one.
Contact the printer maker's support when the first layer changes from print to print while you change nothing, or when the nozzle has scraped the surface.
Next step and related guides
Most readers need one of three follow-ups. Set the nozzle height properly with how to set the Z offset. Fix one bad corner with bed levelling: tramming or a mesh. Learn the right cleaner for your surface in how to clean a 3D printer bed. If the opposite happens and parts will not come off, see removing a print that is stuck to the bed.
If you need the part rather than the practice, the 3D printing service prints PLA and PETG parts from your file.
Sources
Bambu Lab Wiki: First Layer Not Sticking: Causes and Solutions
Bambu Lab Wiki: Identify and Fix First Layer Issues With a Simple Test Print
3D Printing Stack Exchange: Reasons for a PLA print not sticking to bed all the sudden?
3D Printing Stack Exchange: Lines of PLA not sticking to the bed
3D Printing Stack Exchange: Prints falling off the bed towards the end of the print
Ricky Impey on YouTube: How To Get Your 3D Prints To Stick - 7 Top Tips!