PETG settings: start values that work, and what to change when they don't

By Sina Esfahani, OmniTechs · Published 27 November 2026

PETG prints well once you stop treating it like PLA. It wants a hotter nozzle, a warm bed, far less fan and a first layer that is not pressed hard into the plate.

Start from the profile for your exact spool. If you have none, a 240 °C nozzle and a 70 to 80 °C bed sit inside the ranges Prusament, Bambu Lab and Polymaker publish. Keep the fan off for the first layers and around half after that, or lower for strong parts. Limit how much plastic the hotend must melt per second instead of slowing every speed by hand. And put glue stick on a smooth PEI sheet before PETG: Prusa warns that the bond can damage bare smooth PEI.

Set it up in this order:

  1. Load your spool maker's profile; without one, set the nozzle to 240 °C and the bed to 70 to 80 °C on a textured or satin sheet.

  2. Dry the spool first if it pops, crackles or strings heavily (Bambu Lab: 60 to 65 °C for 8 hours); no setting fixes wet PETG.

  3. Part-cooling fan off for the first few layers, then about 50%; 20% or off when the part must not split along its layers.

  4. Max volumetric speed at the maker's figure, or 15 mm³/s if it gives none (Polymaker's limit for PolyLite PETG).

  5. Z-offset: start from your PLA value; if lines come out ridged or the nozzle collects plastic, raise it by 0.02 mm at a time.

  6. Flow ratio 0.95, inside Bambu Lab's 0.93 to 0.96 range for PETG.

  7. Let plate and print cool fully before you remove it; on smooth PEI, apply glue stick first.

Start values per maker

Grades differ: a high-flow PETG melts faster than an older standard one. Use the row for your spool, or that maker's slicer profile.

Published PETG starting values per maker and grade

Values as each maker published them for its own grade, read on 27 November 2026 (Prusa knowledge base, Prusament product page, Bambu Lab wiki, Polymaker wiki). They are the makers' recommendations, not OmniTechs settings, and they do not transfer between grades.
Maker and gradeNozzleBedPart-cooling fanSpeed or flow limit
Prusa knowledge base, PETG in general230 °C first layer, 240 °C after85 °C first layer, 90 °C afterOff for the first few layers, then halfUse the PrusaSlicer profile
Prusament PETG250 ± 10 °C80 ± 10 °C50%Not published
Bambu Lab PETG Basic240 to 270 °C (± 10 °C)60 to 80 °C (textured PEI, smooth PEI or engineering plate)Not in the material tableOuter walls about 90 mm/s if speed changes leave bumps
Bambu Lab PETG HF230 to 260 °C (± 10 °C)60 to 80 °CNot in the material tableUndried spool: Generic PETG HF profile, 220 °C and 16 mm³/s
Polymaker PolyLite PETG (being discontinued)230 to 260 °C70 to 80 °COff to 20%50 to 100 mm/s, at most 15 mm³/s
Polymaker PETG (new high-speed formula)240 to 260 °C60 to 70 °C20 to 60%Up to 300 mm/s; up to 22 mm³/s on a stock Bambu Lab hotend

Read the print: what you see and what to change

Change one thing at a time and reprint the same small part, so you know what worked.

PETG symptoms, causes and fixes

From the Prusa knowledge base, Bambu Lab wiki, Polymaker wiki and accepted 3D Printing Stack Exchange answers, read on 27 November 2026.
What you seeWhat it meansWhat to do
The part splits along its layers or snaps easilyEach layer cooled before it fused to the one belowFan down to 20% or off; nozzle 5 to 10 °C hotter
First layer ridged or wavy; the nozzle drags and collects plasticThe nozzle is too close to the plateRaise the z-offset by 0.02 mm and check again
Corners lift off the plateToo little grip, or the part cools too fastLower the z-offset by 0.02 mm; add glue stick or a brim; keep the bed inside the maker's range
Popping or crackling, bubbles, heavy stringingWater in the filament turning to steamDry the spool before you change any setting
Rough walls or gaps at speed; bumps after overhangsThe hotend cannot melt plastic fast enough, or the speed jumpsLower the max volumetric speed; outer walls about 90 mm/s
Blobs, oozing or a clog with dry filamentToo much flow or too much heat for the speedFlow ratio down to 0.93 or 0.94; nozzle 5 °C cooler
Print fused to a smooth PEI sheetNo release layer between PETG and PEIGlue stick on smooth PEI, or switch to a textured sheet
Filament softens or jams on an enclosed printerThe chamber is too warm for the filamentOpen the door or lift the top glass once the bed is above 60 to 70 °C

Nozzle temperature: hotter for strength, cooler against strings

Heat is a trade-off. Hotter PETG fuses better between layers and gives a tougher part (Prusa); if PolyLite PETG layers still separate with the fan off, Polymaker says go to 250 to 260 °C. Too hot at low speed, and the plastic strings, oozes and builds up on the nozzle (Bambu Lab).

Speed moves the target. At high speed the nozzle has to melt more plastic in less time, so it needs more heat. When you slow down or lower the flow limit, lower the temperature too (Bambu Lab).

To find your value, print a temperature tower across your maker's range in 5 °C steps. Choose the coolest step that still bonds well when you try to snap it.

CNC Kitchen printed one PETG at different hotend temperatures on a Prusa i3 MK2 and measured the strength on a tensile tester.

3D Printing with PETG - How does the printing temperature affect strength? || Setup & Tips (CNC Kitchen)

Part-cooling fan: how much PETG needs

PETG needs some fan for detail and little fan for strength. Cooling keeps small features sharp and reduces strings and blobs. For the toughest part, Prusa turns the fan off. Its default is no fan for the first few layers, then half power.

The right amount depends on the grade. Polymaker's PolyLite PETG loses layer adhesion if it cools too fast, so it runs off to 20%. Its newer high-speed PETG takes more: 20% at a 30-second layer time, rising to 60% at a 10-second layer. If small parts still need cooling, the accepted answer to a much-viewed Stack Exchange question on weak PETG layers suggests starting around 40%.

Where to set it:

  • PrusaSlicer: Filament Settings, Cooling. Set Fan speed Min and Max, and Disable fan for the first X layers.

  • Bambu Studio and OrcaSlicer: the filament preset, Cooling. Set No cooling for the first layers and the fan speed thresholds.

  • Cura: Cooling, Fan Speed and Initial Fan Speed.

Clear PETG is the exception. For transparency, Bambu Lab turns all fans off and prints at about 20 mm/s. The guide to what transparent PETG can look like explains what to expect.

First layer: start from your PLA z-offset, then adjust

Sources disagree here, because they describe different printers and surfaces.

What sources say about the PETG first-layer gap

Positions as published by Prusa and in accepted answers on the 3D Printing Stack Exchange, read on 27 November 2026.
SourceWhat it says
Prusa knowledge base, Live Adjust ZSquish PETG slightly more than PLA, because it tends to lift at the edges
Accepted answer, Stack Exchange, extra Z-offset for PETGNo extra gap was needed over about 8 kg of PETG on several printers
Accepted answer, Stack Exchange, bumpy first layerA bumpy first layer usually means the gap is too small; a commonly quoted extra gap is 0.02 to 0.05 mm
Accepted answer, Stack Exchange, removing PETG from the bedBack the nozzle off until just before adhesion suffers, so the print releases more easily

A safe way through:

  1. Start from the z-offset that gives a good PLA first layer.

  2. Print a single-layer square and look at it. Smooth, flat lines that touch are right.

  3. Ridged lines, a rough surface or plastic piling up on the nozzle: raise the nozzle by 0.02 mm and print again.

  4. Gaps between lines or lifting corners: lower it by 0.02 mm.

In PrusaSlicer the value sits under Printer Settings, General, Z offset; a negative value squishes the first layer more. On Prusa printers you can also tune it live with Live Adjust Z. The z-offset guide covers other printers.

3DJake's video on confusing PETG problems has a chapter on first-layer die swell (PETG swelling as it leaves the nozzle) from 3:33, followed by one on the nozzle dragging through the print.

3 PETG Problems That Might Confuse You... But Are Actually Easy To Fix (3DJake)

Speed: set a flow limit instead of slowing everything

PETG is not slow by nature. The real limit is how much plastic your hotend can melt per second: its volumetric speed, in mm³/s. So cap the filament's max volumetric speed and leave the print speeds alone. That is the fix one of the most-liked replies gives in a long Bambu Lab forum thread on poor PETG quality, and the accepted answer to a Stack Exchange question on PETG speed adds that, with a better extruder, its author printed PETG as fast as PLA.

Bambu Lab gives the formula: volumetric speed = layer height × line width × print speed. A worked example for a 0.4 mm nozzle:

  • At 0.2 mm layers, 0.45 mm lines and 100 mm/s, the hotend melts 0.2 × 0.45 × 100 = 9 mm³/s.

  • With a 15 mm³/s limit, the slicer caps those lines at 15 ÷ (0.2 × 0.45) = about 167 mm/s.

  • At 0.28 mm layers the same limit caps them at about 119 mm/s. Thicker layers hit the limit sooner.

Where to set it:

  • Bambu Studio: edit the filament preset, Filament tab, Max volumetric speed.

  • OrcaSlicer: filament settings, Filament, Volumetric speed limitation, Max volumetric speed.

  • PrusaSlicer: Filament Settings, Advanced, Max volumetric speed. Print Settings, Speed has the same field; the lower value wins.

Bambu Lab recommends a flow ratio of 0.93 to 0.96 for PETG: below that the layers weaken, above it the nozzle oozes or clogs. Its default for PETG Basic is 0.95. If walls show bumps where the speed jumps after an overhang, keep outer walls around 90 mm/s. For flow problems beyond that, calibrate the flow ratio.

Bed and plate: grip while printing, release when cool

Published beds run from 60 °C (Bambu Lab, Polymaker's new PETG) to 90 °C (Prusa). Bambu Lab does not recommend its Cool Plate for PETG. It prefers an enclosed printer, because cold air weakens PETG's layers, but once the bed is above 60 to 70 °C it advises opening the door or lifting the top glass, so the warm chamber does not soften the filament before the nozzle.

PETG can bond too well. The makers agree on how to keep it releasable:

  • Use a textured or satin sheet (Prusa). On smooth PEI, apply glue stick first as a separator; Bambu Lab adds that glue at a 60 to 80 °C bed makes removal easier and protects the plate.

  • Do not wipe the plate with isopropyl alcohol before PETG: it can make adhesion too strong. Prusament prefers window cleaner on a paper towel, wiped on while the bed is cold.

  • Wait until plate and print are at room temperature before you remove it (Polymaker, Bambu Lab).

The guide to heated bed temperature for PLA and PETG explains what too hot looks like. If a part is already stuck, follow the guide to removing a print stuck to the bed.

When to stop tuning

  • The spool is wet. Bambu Lab calls PETG highly hygroscopic and links obvious stringing and bubbles to damp filament. No setting fixes that; dry it as the filament drying chart gives for your brand.

  • Your hotend has a PTFE liner down to the nozzle. E3D gives its PTFE-lined Lite6 a limit of 240 °C, and Creality warns that a standard PTFE tube degrades above 240 °C and releases toxic fumes. Stay at the bottom of the PETG range or move to an all-metal hotend; the guide to all-metal or PTFE-lined hotends explains the difference.

  • Nothing helps and the extrusion looks thin. In one Stack Exchange thread, poor PETG prints turned out to be a damaged nozzle with a widened hole, probably from cleaning. A replacement nozzle fixed it.

  • The sheet is torn. If PETG has pulled pieces out of a PEI surface, that sheet will keep failing; replace it.

If your settings now work but fine hairs remain, diagnose PETG stringing one variable at a time. If layers still split with the fan low, the guide to layer separation goes deeper. Still deciding on the material? Compare PLA or PETG for your part.

If you need the part rather than the practice, OmniTechs prints PETG parts from your file.