PLA vs PLA+: what the plus changes and when it is worth buying

By Sina Esfahani, OmniTechs · Published 27 November 2026

PLA+ is a sales name, not a material standard. Each filament maker decides what goes into its "plus", "Pro" or "Tough" PLA, and none has to say which additive it used.

What the plus buys you is toughness. On Bambu Lab's and Polymaker's own datasheets, the tougher grades absorb 5 to 12 times more impact energy than the same maker's standard PLA. They do not resist heat better: all five sheets put the heat deflection temperature between 55 and 61 °C. Tensile strength, the pull a test bar takes before it breaks, stays the same or drops.

Buy a plus grade for parts that must survive drops, snap fits and clamping. For heat, sun or a stiff bracket, it buys you nothing.

Decide in this order:

  1. Name the failure you want to avoid: shattering on impact calls for a plus grade; softening in heat or sun calls for PETG or ASA instead.

  2. Download the technical datasheet for the exact grade and version; a shop page is not a datasheet.

  3. Compare notched impact strength within one maker and one test method; the plus grades below reach 5 to 12 times the standard value.

  4. If the part is loaded across its layers, check the upright (Z) tensile strength as well.

  5. Check the heat deflection temperature: within a few degrees of 57 to 60 °C means no gain in heat resistance.

  6. Print from the spool's own range, not your PLA profile: Bambu Studio starts PLA Tough+ at 245 °C, 25 °C hotter than PLA Basic.

Is a plus grade worth it for your part?

What a plus grade changes, by the job your part has to do

Summary of the five Bambu Lab and Polymaker datasheets compared below and of Prusa's PLA guide, read 27 November 2026.
Your part has toPlus grade?What the makers' datasheets show
Survive drops, snap fits or clampingYesNotched impact strength 5 to 12 times the same maker's standard PLA
Carry a steady load or stay stiffNo, often worseFlat tensile strength equal or lower; Bambu Lab PLA Tough+ is weaker between layers (20.9 against 31 MPa)
Stay in a car or near heatNoHeat deflection 55 to 61 °C, the same band as standard PLA
Live outdoors in the sunNoNone of these makers claims better UV resistance; Prusa says PLA degrades under UV light
Look silky, matte or filledA different productThose grades change the surface, not the toughness

Silk, matte and filled PLA are covered in silk, matte and speciality PLA.

What does PLA+ actually mean?

You will see the same idea sold as PLA+, PLA Plus, PLA Pro, Tough PLA or Impact PLA. Polymaker describes these grades as PLA with added plasticisers, impact modifiers or nucleating agents. Those additives let the part absorb a blow instead of shattering. The base polymer is still PLA, so it still softens where PLA softens: Polymaker gives its PolyMax PLA about the same heat resistance as regular PLA, about 60 °C.

The safety data sheets show how much is added. Bambu Lab's PLA Basic is 95 to 99% polylactic acid with 1 to 5% additive. Its PLA Tough+ is 80 to 90% polylactic acid with 10 to 20% additive. Neither sheet names the additive.

Plain PLA is not pure either. An accepted answer on the 3D Printing Stack Exchange points out that ordinary PLA already carries colourants and other additives, and that "plus" says nothing about which ones or how much.

One maker can even sell several plus grades with different aims. Polymaker calls PolyLite PLA very rigid with very low impact resistance, PolyMax PLA extremely ductile, and PolyLite PLA Pro a combination of rigidity and high impact strength.

What the datasheets show

Each row below is one datasheet. Both makers print solid test bars and test them to the same ISO methods, so rows from the same maker can be compared.

Standard and tougher PLA grades on their makers' own datasheets

Values as printed on each maker's datasheet (ISO 75, ISO 527, ISO 179), read 27 November 2026. Bambu Lab annealed and dried its bars at 50 to 55 °C for 8 hours before testing; Polymaker's sheets mention no annealing. Test-bar values, not ratings for your part.
Grade and datasheetHDT at 0.45 MPa (°C)Tensile strength, flat (MPa)Tensile strength, upright (MPa)Notched Charpy impact, flat (kJ/m²)Nozzle range (°C)
Bambu Lab PLA Basic, TDS V3.05735317.9190 to 230
Bambu Lab PLA Tough+, TDS V3.06134.920.972.3220 to 250
Polymaker PolyLite PLA, TDS V5.46052.340.53.3190 to 230
Polymaker PolyLite PLA Pro, TDS V5.65949.836.517.1190 to 230
Polymaker PolyMax PLA, TDS V5.45541.332.438.9190 to 230

Three things stand out:

  • Impact strength is the big change. PLA Tough+ absorbs about nine times the notched impact energy of PLA Basic. PolyLite PLA Pro reaches about five times the value of PolyLite PLA, PolyMax PLA about twelve times.

  • Strength does not rise with it. PLA Tough+ matches PLA Basic flat (34.9 against 35 MPa), but upright, where the layers are pulled apart, it reaches only about two thirds (20.9 against 31 MPa). PolyMax PLA is weaker in tension than PolyLite PLA. "Tough" means the part absorbs more energy before it breaks, not that it carries more load.

  • The two makers' numbers do not line up. Their standard PLAs differ by more than a factor of two in notched impact (7.9 against 3.3 kJ/m²), and only Bambu Lab says it anneals its test bars.

Grades also change. Polymaker announces that PolyLite PLA Pro will be discontinued by the end of 2026 and replaced by Polymaker PLA Pro, which its summary table lists at 20.76 kJ/m². Check which grade is on your spool.

CNC Kitchen tested regular against modified PLA, using the same Polymaker PolyLite and PolyMax filaments as in the table, for printability, strength, stiffness, impact resistance and behaviour under heat.

How much STRONGER is PLA+ really? (CNC Kitchen)

Worked example: two datasheets, one dropped clip

You want a clip for a bag strap. It gets dropped and squeezed, never heated. You have PolyLite PLA and wonder whether PolyMax PLA is worth it.

  1. Same maker, same test? Yes: both Polymaker sheets use notched Charpy to ISO 179 on solid bars printed at 230 °C. The rows are comparable.

  2. Impact: 38.9 against 3.3 kJ/m². PolyMax PLA absorbs about 12 times the energy before a notched bar breaks.

  3. Strength: 41.3 against 52.3 MPa flat, about 21% lower; 32.4 against 40.5 MPa upright.

  4. Heat: 55 against 60 °C heat deflection, 5 °C lower.

Verdict: PolyMax PLA for the clip, and keep it out of a hot car. For a bracket that holds a shelf, the same numbers point the other way.

With other brands, watch for four traps:

  • A shop page is not a datasheet. On 27 November 2026, eSUN's PLA+ and standard PLA product pages printed the identical property table, and the PLA+ page linked the PLA documents. Those pages show no difference at all.

  • Pages from one maker can disagree. Polymaker's PolyLite PLA Pro product page gives 190 to 220 °C and 30 to 70 mm/s; its newer V5.6 sheet gives 190 to 230 °C and 50 to 200 mm/s. Use the newest dated sheet.

  • Charpy is not Izod, and the notch matters. Bambu Lab's own PLA Basic sheet lists 26.6 kJ/m² without a notch and 7.9 kJ/m² with one. Compare the same standard with the same notch only.

  • Read how the bars were made. Annealing, print temperature and infill all move the result.

The datasheet comparison of 17 sheets explains in more depth why rows from different makers cannot be compared directly.

CNC Kitchen also tested a modified PLA sold as a replacement for ABS, which shows how to hold a toughness claim against measurements.

What is TOUGH PLA?! Testing AzureFilm Strongman™ PLA (CNC Kitchen)

Which settings change for a plus grade?

Start from the spool, not from your PLA profile. Bambu Lab gives 220 to 250 °C for PLA Tough+ against 190 to 230 °C for PLA Basic, and Bambu Studio's own profiles print them at 245 °C and 220 °C.

Polymaker advises printing PolyLite PLA Pro and PolyMax PLA slower than standard PLA, with a maximum volumetric speed (the most plastic the hotend may melt per second) of 15 mm³/s. At that flow it raises the nozzle to 220 to 230 °C. With a 0.4 mm nozzle, 0.45 mm lines and 0.2 mm layers, 15 mm³/s works out at about 167 mm/s, using Bambu Lab's formula: layer height × line width × speed.

Where to set that cap:

  • Bambu Studio and OrcaSlicer: edit the filament preset, Filament tab, Max volumetric speed (OrcaSlicer groups it under Volumetric speed limitation).

  • PrusaSlicer: Filament Settings > Advanced > Max volumetric speed. PrusaSlicer uses the lower of this and the print profile's value.

The maker's range is a starting point, not a promise. A Stack Exchange user got heavy stringing with an Inland PLA+ inside the maker's own 215 to 225 °C. The accepted answer: the maker's test printer is not yours, so use the temperature that works on your machine; a second answer adds that print speed shifts it. Print a temperature tower for each new spool.

Dry a spool that has been open for a while: Polymaker gives 55 °C for 6 hours for PolyLite PLA Pro, Bambu Lab 55 °C for 8 hours for PLA Tough+ in a forced-air oven. The filament drying chart lists other materials.

When a plus grade will not save the part

  • It bent in the heat. A PLA+ part deforms where standard PLA does, for example on a sunny dashboard. Reprinting in PLA+ will not help; see PLA in a hot car for materials that will.

  • It has to live outside. Prusa states that PLA degrades under UV light and is not suited to outdoor use, and none of the makers above claims a plus grade changes that. See the best filament for outdoor use.

  • It has to stay stiff or carry load across layers. A ductile grade such as PolyMax PLA bends instead of breaking, and PLA Tough+ is weaker between layers. Wall count and print direction matter more here; see how strong 3D-printed parts are.

For reading one sheet against the job your part has to do, the guide to reading a PETG material datasheet uses the same method and works for PLA too.

If you need the part rather than the material experiment, the 3D printing service prints PLA and PETG parts from your file and confirms the exact grade in the quote.